Using Rheology to Evaluate Polymer Degradation

Keywords: Oxidation, Polymer, Degradation, OWCh, Chirps

RH167

Abstract

Polymer degradation in air at high temperatures can be studied using rheology and the Waters TA Instruments™ ARES-G3™ Rheometer paired with the Forced Convection Oven (FCO). Rheology is a useful method to examine polymers because the rheological properties are sensitive to molecular weight and viscosity changes, which can impact processing. The FCO can switch gas sources quickly without changes in temperature to vary the oven’s atmosphere. This note will describe the rheological changes of polyethylene with a short exposure to air and polystyrene under continuous exposure to air. Fast frequency chirps, based on optimally windowed chirps [1,2], allow for a fuller characterization of the flow curve via the Cox-Merz rule and of the frequency crossover to reveal information about the changes in average molecular weight (MW) and molecular weight distribution (MWD).

Introduction

The FCO is a gas convection oven that excels in fast temperature changes, temperature stability, and gas exclusion. Gas is forced into the oven chamber with the sample after passing over heating elements to pre-heat the gas to the desired temperature. The instrument can be configured with gas and air inputs so that the oven atmosphere can be switched quickly from pure nitrogen to dry air without temperature changes. The FCO can quickly change the gas composition of the oven by forcing the purge of the oven, which allows for the following study.

Fast frequency chirps, available on the Discovery™ Hybrid Rheometers and ARES-G3 Rheometer, allow for fast measurements of the viscoelastic properties across a wide set of frequencies. Polymers will react rapidly with air at high temperatures, but the chirp takes only a single period of the lowest frequency to gather the data needed to make the measurement.

The data generated from a chirp can be transformed via the Cox-Merz rule, which relates the complex viscosity to the shear viscosity and the angular frequency to the shear rate. This transformed data can then be fit to flow models such as the Williamson model to determine zero-shear viscosity and other parameters that indicate the shear thinning of the material. The zero-shear viscosity relates to the average MW of the material, and the shear thinning is indicative of MWD.

A crossover point is defined as the modulus and frequency where the storage and loss modulus are equivalent on a modulus vs. frequency plot and can be determined with chirp data. This crossover point is also the point where tan(δ) is unity as tan(δ) is G”/G’. The crossover frequency and modulus also have known relationships with the MW and MWD, respectively [3].

Experimental

Linear low-density polyethylene (LLDPE) pellets were loaded onto 25 mm parallel plates in the ARES-G3 FCO, melted at 130 °C and trimmed. The oven temperature was then raised to 200 °C under nitrogen atmosphere while maintaining 0 ± 0.1 N of axial force. Fast frequency chirps were used to analyze the sample from 0.05 to 50 Hz at 1% strain amplitude with a 10 s relaxation break between chirps. The chirps were tested with 1 s baseline, 0° phase shift, and 15% tapering parameter.

A polyethylene sample was measured for 10 minutes under nitrogen purge then the atmosphere was switched to air for 60 s then switched back to a nitrogen environment. Chirp data collection continued for 50 minutes. Another sample of the same polymer was measured without any exposure to air after 10 minutes to use for comparison as a control sample.

After each experiment, the polyethylene samples were cooled down below the melt temperature (~100 °C) and allowed to solidify. The solid polymer discs were separated from the parallel plates intact for observation.

The same chirp protocol and geometry were used on a polystyrene sample. The environment started in nitrogen at 230 °C where the sample was loaded and trimmed. The environment started as nitrogen, switched to air, then back to nitrogen for 10 minutes in each segment for a ~30-minute experiment.

Results and Discussion

The overall polyethylene results can be seen in Figure 1. Before 10 minutes, the control and exposed sample show very good agreement for complex viscosity (η*) and tan(δ). The two samples begin to deviate after the 60 s air exposure. The control sample shows very little change over the course of the experiment, indicating a very stable sample due to the nitrogen atmosphere of the FCO.

After exposure to air, the polymer η* increases and tan(δ) decreases at low frequencies in a nitrogen environment with no further air exposure. The samples after the test are shown in Figure 2. The control sample has the same color as the pellets loaded into the instrument at the start of the test. The exposed sample has a brown edge that was exposed to air and oxidized.

Figure 1. A. The η* (solid lines) and tan(δ) (dotted lines) for the polyethylene control sample (blue) and exposed sample (red) from chirps collected for one hour and approximately every 40 s. The control and exposed measurements overlap well for the first 10 minutes of nitrogen environment and begin to deviate from each other after the air exposure. Red arrows on the plot indicate the direction of the change with time for the exposed sample. The control sample shows little change, as expected, while the exposed sample continues to change well after the 60 s exposure event.
Figure 1. A. The η* (solid lines) and tan(δ) (dotted lines) for the polyethylene control sample (blue) and exposed sample (red) from chirps collected for one hour and approximately every 40 s. The control and exposed measurements overlap well for the first 10 minutes of nitrogen environment and begin to deviate from each other after the air exposure. Red arrows on the plot indicate the direction of the change with time for the exposed sample. The control sample shows little change, as expected, while the exposed sample continues to change well after the 60 s exposure event.
Figure 2. Control and Exposed samples of polyethylene cooled and removed from the plates. The exposed sample shows a brown edge while the control sample shows no visible change from the color of the pellet material or the material directly under the plates and not exposed to the oven atmosphere.
Figure 2. Control and Exposed samples of polyethylene cooled and removed from the plates. The exposed sample shows a brown edge while the control sample shows no visible change from the color of the pellet material or the material directly under the plates and not exposed to the oven atmosphere.

The center of the exposed sample is covered by the 25 mm plates and shows no visible evidence of a reaction with air. This observation is important as it indicates that all the changes observed in the rheological data are coming from the edge of the sample. The sample edge contributes most to the overall torque signal in the parallel plate configuration but the contributions from under the plate are not negligible. The measured system is a combination of the oxidized edge and unreacted polymer.

Figure 3 shows time traces for individual frequencies pulled from the data in Figure 1. The control and exposed sample match for the first 10 minutes and deviate after the exposure to air (red line on each plot). Interestingly, η* and tan(δ) signal do not begin significantly deviating right away at 0.05 Hz as shown in Figure 3a. There is a short time (15 min) after the exposure where there is only a small deviation in phase angle and complex viscosity, followed by a much faster rate of change around 15 minutes after the exposure event. A typical experiment without chirps would be done at one frequency and would look much like Figure 3a. The likely conclusion would be that there is an induction time or delay from when the exposure happened to when the reaction of the polymer started progressing. We can see, however, that there are immediate signs of exposure at the higher frequencies provided by the fast frequency chirp experiment. To obtain the same frequency data from a typical experiment, multiple sample loadings would be required.

Figure 3b shows the time trace for 0.25 Hz and there is a clear immediate drop in η* and tan(δ) followed by an increase in η* and a more rapid drop in tan(δ). The data in Figure 3c and 3d also show an immediate drop in η* followed by a small increase or leveling off for 5 Hz and 50 Hz, respectively. The tan(δ) for these two frequencies also shows a very small decrease over time compared to the data at lower frequencies.

The control sample shows a very stable signal throughout the experiment, indicating all observed changes after the exposure time are due solely to the short exposure to air. There are minor drifts in the η* signal for the control that likely relate to the meniscus or edge of the sample relaxing and slightly changing shape. This change only impacts effectively how much sample is being probed under the plate volume so only the torque and therefore modulus or η* are affected while the phase angle is entirely unchanged.

While trends can be viewed one frequency at a time, another way to probe the reaction is to fit the resulting curves to determine properties that relate to the MW. As previously discussed, the reaction appears to only occur at the edge exposed to the atmosphere, so the result is a convolution of the reacted sample and unreacted sample under the plate. Nonetheless, the Williamson model (Equation 1) can be fit to viscosity (η) vs. shear rate (γ̇), which can be obtained via the Cox-Merz transformation. The Williamson model has zero-shear viscosity η0, consistency k, and rate index parameter ni as fitting parameters.

A simple modulus crossover analysis determines the frequency and modulus where tan(δ) is unity. The point at which tan(δ) is one is also where the storage and loss moduli are equivalent, which is why it is called the modulus crossover. The data in this note reliably had a single crossover point.

Both the Williamson and crossover point give clues to what may be happening to the polymer after it was exposed to oxygen. The η0 relates to the average molecular weight (MW) [3]. Increasing η0 indicates a higher average MW. The transition from the zero-shear plateau also gives clues to the molecular weight distribution (MWD) [3]. A sharp transition and broad zero-shear plateau are indicative of a narrow distribution while a short plateau and earlier shear thinning is associated with a broad MWD. The chirps are limited in duration to capture the progression of the reaction so the fit value for η0 is the best indicator of the plateau value. In a stable system, it would be important to capture a segment of the plateau to make the determination. The onset of shear thinning can be tracked with ni and k. Lower rate index values and higher consistency values indicate earlier shear thinning and a narrow plateau associated with a broader MWD.

The results of the Williamson model fitting are shown in Figure 4. Before exposure to air (vertical red line) the values are consistent and unchanging. After exposure, η0 remains largely stable for nearly 15 minutes and the consistency largely tracks with the η0 except for a small initial jump. The rate index shows an immediate small drop and then a faster drop with as the η0 begins to rise. The data in Figure 4 indicate that there is some induction time for the average MW, while the MWD begins changing immediately but accelerates after the apparent induction time.

The crossover modulus data in Figure 5 tells a similar story to the data from the Williamson model. The crossover modulus is related to the MWD and the crossover frequency is an indicator of the average MW [3]. Lower crossover frequency indicates higher average MW while lower crossover modulus indicates a broader MWD.

Figure 4. Williamson fit results for each chirp vs. the time when the chirp started. The red vertical line indicates when the sample was exposed to 60 s of air atmosphere before switching back to nitrogen. These results show an apparent increase in MW and broadening of the MWD due to the exposure.
Figure 4. Williamson fit results for each chirp vs. the time when the chirp started. The red vertical line indicates when the sample was exposed to 60 s of air atmosphere before switching back to nitrogen. These results show an apparent increase in MW and broadening of the MWD due to the exposure.
Figure 5. Crossover modulus analysis results vs. the time when the chirp started. The blue squares are the crossover frequency, and the green triangles are the crossover modulus. The red line indicates when the sample was exposed to 60 s of air atmosphere before switching back to nitrogen.
Figure 5. Crossover modulus analysis results vs. the time when the chirp started. The blue squares are the crossover frequency, and the green triangles are the crossover modulus. The red line indicates when the sample was exposed to 60 s of air atmosphere before switching back to nitrogen.

The crossover frequency shows a small initial change but stays largely stable for about 15 minutes after exposure, then begins to drop. This drop in crossover frequency and modulus indicates the same thing as the η0 and ni from the Williamson model fit: an initial induction time for any change in the average MW indicator with an immediate initial change in the indicator for MWD that keeps changing throughout the rest of the experiment.

The data from the polyethylene sample show that after a short exposure to air at high temperatures there seem to be reactive sites generated on the surface of the polymer that continue to react and change the polymer architecture well after the exposure. The rheological signatures indicate an increasing MW and broadening MWD. The data indicate an immediate change in the distribution which may be related to the edge reacting while the material under the plate is protected. The apparent induction time for the average MW changes seems consistent across the low frequency η*, the fitted η0 value from the Williamson model, and the crossover frequency. Measurements of the samples in Figure 2 show that there is no significant dimensional or weight difference indicating the modulus and complex viscosity changes are from material property changes rather than the reaction changing the dimension of the sample.

The Williamson fit and crossover point analysis is expanded to a polystyrene sample where the same tools show a very different trend. Polystyrene appears only to change while exposed to air and the MW appears to decrease while in the air environment. While the atmosphere is nitrogen the polymer appears stable and unchanging. The whole series of chirps from this experiment is shown in Figure 6. There are three 10-minute segments in this experiment. The first is a set of chirps in a nitrogen environment showing a stable system, the next in air showing the sample reacting with air, and then another nitrogen segment showing a changed but stable system.

Figure 6. Complex viscosity and tan(δ) of polystyrene in nitrogen (a), air (b) and back to nitrogen (c) for 10 minutes in each segment. The sample is unchanged in the initial and final nitrogen environment. The η* decreases and tan(δ) slightly increases at all frequencies with time in air.
Figure 6. Complex viscosity and tan(δ) of polystyrene in nitrogen (a), air (b) and back to nitrogen (c) for 10 minutes in each segment. The sample is unchanged in the initial and final nitrogen environment. The η* decreases and tan(δ) slightly increases at all frequencies with time in air.

Crossover analysis and Williamson model fit results in Figures 7 and 8 also show that the material is stable in nitrogen and only changes in air but primarily it is the MW that is affected. Figure 7 shows the crossover frequency and zero-shear viscosity which are strong indicators of the average MW and they show fast and dramatic changes in air while there is not an obvious change in the nitrogen environment before and after the air segment.

Figure 7. Plot of the crossover frequency, η0, and the status of the gas in the FCO for polystyrene. Status 1 is air and 2 is nitrogen. An increase in the crossover frequency and decrease in η0 both indicate a decrease in average MW. The material is stable while in nitrogen and both signals indicate a decreasing MW in air.

Figure 7. Plot of the crossover frequency, η0, and the status of the gas in the FCO for polystyrene. Status 1 is air and 2 is nitrogen. An increase in the crossover frequency and decrease in η0 both indicate a decrease in average MW. The material is stable while in nitrogen and both signals indicate a decreasing MW in air.

Figure 8. Plot of crossover modulus, ni, k, and gas status in the FCO for the polystyrene sample. These parameters are indicators of MWD and show only small changes during air exposure.

Figure 8. Plot of crossover modulus, ni, k, and gas status in the FCO for the polystyrene sample. These parameters are indicators of MWD and show only small changes during air exposure.

The indicators of MWD in Figure 8 show much less change compared to the polyethylene sample and are somewhat conflicting. The Williamson model fit parameters k and ni both decrease when exposed to air but otherwise are stable in nitrogen. The crossover modulus slightly increases then decreases during the air step. The changes are all relatively small and conflicting, indicating little change in the MWD.

The polystyrene shows very different behavior compared to the polyethylene. The polystyrene data indicate a decreasing MW without large impacts on the MWD while the polyethylene appears to increase in MW with a changing MWD. The polystyrene also appears to require constant exposure to oxygen/air for the reaction to progress. Chain scission or a breakdown of the longer chains appears to be occurring. Only a short exposure to air is enough to create reactive sites for the polyethylene reaction to continue well after the exposure. Crosslinks or otherwise increase the MW.

Conclusions

The Forced Convection Oven on the ARES-G3 Rheometer utilizes a pure nitrogen environment and has the ability to pre-heat the incoming gas into the test chamber. The design of the oven allows for fast atmosphere changes around the polymer without any change in temperature. These features are ideal for studying degradation of polymers with rheology.

The application of fast frequency chirps based on optimally windowed chirps allows for a fuller characterization of the rheology. Chirps effectively produce a full frequency sweep within the period of the lowest frequency probed. The data produced allow for more assessment of trends in modulus and phase angle than a single frequency test would give.

The trends of the frequency sweeps can be fit to models such as the Williamson model as in this note or others to predict low shear viscosity that relates to molecular weight or parameters that characterize the shear thinning which relates to the molecular weight distribution.

The same data from chirps that can be used for shear viscosity models can also be used to produce storage and loss modulus data. A modulus crossover point analysis can be used to determine trends in molecular weight and molecular weight distribution from the crossover frequency and crossover modulus.

The temperature system combined with fast frequency chirps in this note allowed for characterization of MW and MWD indicators in two ways for polyethylene and polystyrene. Polyethylene after a short 60 s exposure to air at high temperatures continued to react for 50 minutes after the exposure with an apparent increase in MW and broadening of the MWD. Polystyrene required continued exposure to air for degradation to progress and showed decreasing MW with little change in the MWD.

References

  1. Geri, M., et al., Phys. Rev. X 8, 041042, 2018
  2. Hudson-Kershaw, R. et al., M., J. Non-Newton. Fluid Mech, 333, 105307, 2024
  3. Aly Frank Ph.D. “Introduction to Polymer Melt Rheology and Its Application in Polymer Processing” tainstruments.com https://www.tainstruments.com/applications-notes/introduction-to-polymer-melt-rheology-and-its-application-in-polymer-processing/ (accessed June 16th, 2026)

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Kevin Whitcomb, Ph.D, Principal Applications Scientist.

Waters, TA Instruments, ARES-G3, and Discovery are trademarks of Waters Corporation or its affiliates.

Click here to download the printable version of this application note.