Thermo-Physical and Dielectric Properties of Thermal Management Materials

Keywords: thermal conductivity, insulation, mechanical strength, rheology, dielectric, PCMS, TIMS

TPP037

Abstract

Thermal management materials (TMMs) are becoming increasingly important in the electronics industry, providing control over the dissipation of heat in devices. A number of design strategies have produced a variety of TMMs. While the materials landscape is vast, there are fundamental properties of these materials that need optimized or modified to make them fit for function. One such class of materials are thermal interface materials (TIMs). While various designs exist they generally all possess poor electrical conduction, good thermal conductivity, and various but well-defined levels of strength. This note presents a workflow to characterize the thermal conductivity, insulative properties, and shear mechanical strength of three different TIMs as a function of temperature. A simple strategy to quickly identify the appropriate material for an application will then be discussed.

Introduction

The rapid advancement of electronic technologies has led to increasing device miniaturization, higher power densities, and greater functional integration. As a result, efficient thermal management has become a critical factor governing device performance, reliability, and lifetime. In modern electronic devices, a substantial portion of the total thermal resistance arises not from the bulk materials themselves but from the interfaces between heat-generating and heat-dissipating components such as heat spreaders or heat sinks. Among the various strategies developed to manage interfacial heat transfer bottlenecks, thermal interface materials (TIMs) play a central and indispensable role [1]. This can be seen in the TIMs market projections with anticipated growth from $4.13 billion in 2023 to $9.91 billion by 2032, reflecting a compound annual growth rate (CAGR) of 10.2% [2].

There are various material classes used to design TIMs, including polymer-based, carbon-based, metal-based, and phase change materials (PCMs) [3]. When designing TIMs, requirements must be met, such as sufficient thermal conductivity, mechanical compliance with sufficient stiffness for handling and processing, electrical insulation, and thermal stability [4,5]. Another key consideration is easy application of the TIM. A strategy commonly employed for polymer-based and PCM TIMs is to form them into pads or sheets. Compared to low compliance designs such as greases, pads can be easier to apply and are more robust with adequate compliance.

Polymer-based TIMs generally utilize an elastomeric network with various additives to modify properties such as thermal conductivity and electrical insulation. An example of this type of TIM is a silicone-based material that is highly filled with ceramic additives. In this TIM design, the silicone elastomer acts as a binding material for the additive and provides mechanical compliance, ease of processing, and ease of application. The highly filled ceramic increases the thermal conductivity (λ) above silicone’s relatively low values (λ < 0.2 W/m*K). Use of ceramics in place of higher electrically conductive metallic or carbon-based fillers also maintains sufficient electrical insulation in the material [6].

PCM TIMs are generally designed with phase change materials such as paraffins, synthetic hydrocarbons, or fatty acids. This medium will have a transition point, typically around 40-70 °C where it changes phase or melts. The introduction of a phase transition with an associated latent heat is useful for high transient heat flux systems where temperature spikes can be absorbed by the PCM. This significantly reduces or eliminates damage between components, thus maintaining device performance and lifetime.

Thermally conductive additives are dispersed in the TIM for enhanced thermal conductivity and uniform heat transfer. To provide structural integrity along with ease of handling, a polymeric binder or support scaffold is incorporated. Combined, this produces a material that can be easily placed between electronic components. Subsequent heating above the phase change temperature induces pad softening or partial melting, which allows the material to flow into micro-voids within the components. This filling of microscopic gaps and surface irregularities allows for a uniform coating of the components, which reduces thermal resistance and improves heat transfer compared to traditional thermal pads and greases [7,8].

A workflow will be presented for the characterization of thermal conductivity, dielectric, and shear rheological properties of thermal management materials (TMMs). The analysis utilized a Waters TA Instruments™ FOX 50 heat flow meter (HFM) for thermal conductivity measurements. Rheological and dielectric measurements were measured on a Waters TA Instruments Discovery™ HR 30 stress-controlled rheometer equipped with the dielectric accessory. The analysis will focus on the thermal conductivity (λ), dielectric constant (κ), and shear storage modulus (G′) as a function of temperature. An analysis strategy to quickly identify the appropriate material for an application will be presented based upon the measured properties.

Experimental

Materials

For this work, a silicone-based TIM with ceramic additives was analyzed in addition to a PCM TIM and silicone foam pad control sample. This foam pad is designed for thermal runaway control but is not considered a TIM as it is not designed to increase thermal conductivity. The foam pad material was chosen to show the low-end sensitivity of the instrumentation and can be contrasted to the filled silicone TIM. All materials used were commercially available and used as received. The filled silicone-based TIM contained Boron Nitride (BN) as the ceramic filler. The PCM TIM is composed of two additive-infused PCM layers with a polyimide thin film in between. The silicone foam (SF) consisted of a micro-cellular structure. The materials will be referred to as BNS TIM, PCM TIM, and SF TMM, respectively.

Thermal Conductivity

A FOX 50 HFM was utilized for thermal conductivity measurements. Samples were prepared as 50 mm diameter single layer disks. The HFM measurement consists of a vertical configuration where the sample disk is held under compression between two polished metal surfaces. Heat flows from the upper heated surface to the lower surface, which is part of a calibrated heat transducer. By holding the upper and lower surfaces at a temperature differential, an axial temperature gradient is established (Figure 1 [9]). A 1 °C difference between upper and bottom plates was used in this work. The λ is measured utilizing the temperature difference (ΔT) across the sample of known thickness (L) along with the heat flux (q) output from the heat flow transducer (Equation 1). The λ was measured from 0-80 °C in 10 °C temperature increments.

Figure 1. Schematic of FOX 50 guarded HFM test configuration. Thermal conductivity calculation shown in Equation 1.
Figure 1. Schematic of FOX 50 guarded HFM test configuration. Thermal conductivity calculation shown in Equation 1.

Rheo-Dielectric

An HR 30 rheometer was equipped with the dielectric accessory, shown in Figure 2, and used to measure the shear mechanical and dielectric properties as a function of temperature and frequency. All measurements were performed with 25 mm parallel plates. To negate any thickness differences between samples, the axial force was controlled to 1 ± 0.1 N. Temperature ramps were run from 0–100 °C with a mechanical oscillation frequency of 1 Hz at 0.01% strain and the dielectric properties were simultaneously measured at 1 V and 1 MHz frequency. Dielectric frequency sweeps were run from 100 Hz – 1 MHz at 1 V and 40 °C to examine the dielectric properties at a common operating temperature.

Figure 2. (a) Rheo-dielectric configuration on an HR 30 rheometer with environmental test chamber (ETC) for temperature control (b) Schematic of rheo-dielectric configuration components
Figure 2. (a) Rheo-dielectric configuration on an HR 30 rheometer with environmental test chamber (ETC) for temperature control (b) Schematic of rheo-dielectric configuration components

Results and Discussion

Thermal Conductivity

One of the most important properties to consider for TMMs is thermal conductivity, λ. In TIM pads, this is generally achieved by adding highly thermally conductive additives to a lower thermally conductive polymer scaffold or structural network. This generally leads to TIMs with λ values ranging from ~0.5 – 10+ W/m*K [10]. Figure 3 shows the temperature dependent λ behavior of the three materials as a function of temperature from 0 – 80 °C. The BNS TIM with BN ceramic filler shows the highest λ of the three materials tested.

Figure 3. Thermal conductivity as a function of temperature for the three TMM materials
Figure 3. Thermal conductivity as a function of temperature for the three TMM materials

The BNS λ decreases weakly with temperature from 4 – 3 W/m*K. The ceramic filler provides a 15 – 20x increase in λ compared to the silicone matrix (λ ~ 0.2 W/m*K) with no filler. The decreasing and then plateauing λ from low to higher temperature is a commonly observed result for BN-filled polymeric TIMs [11]. BN thermal transport relies heavily on phonon transport and as temperature increases, the phonon-phonon scattering increases and reduces heat transport efficiency, thus slightly reducing λ. This dependence is generally weak however and tends to plateau within certain temperature ranges.

The PCM TIM exhibits an increasing λ (0.2 – 0.6 W/m*K) trend with temperature. From the PCM TIM data set in Figure 3, λ begins increasing after 20 °C. This temperature is consistent with the onset of the phase transition determined from differential scanning calorimetry (DSC) and thermo-mechanical analysis (TMA) [12]. When the transition is reached and the material begins to soften/melt, the increase in λ can be attributed to several phenomena such as increased interfacial wetting. This increased interfacial wetting causes homogenous surface coverage and elimination of air gaps, acting synchronously to provide a larger effective contact area and produces improved heat transfer pathways. The PCM λ is lower compared to the BNS TIM but is consistent with commonly used PCM materials with little thermally conductive filler [13]. In addition, the PCM TIM is a layered structure with a polyimide support film which has an inherently low λ. The phase transition for PCMs has an associated latent heat which can serve to absorb temperature spikes during application and protect device components.

The SF TMM showed a low and very weak temperature dependent λ (0.14 – 0.16 W/m*K). This is anticipated as the material is designed to be thermally and electrically insulating. The microcellular structure produces air pockets throughout the material which significantly increases thermal resistance and lowers the λ below silicone’s common value of ~0.2 W/m*K. This material shows the low-end sensitivity of the FOX 50 instrument and its ability to characterize a wide range of TMMs.

Rheo-Dielectric

In addition to thermal properties, the electrical and mechanical properties of TMMs are also key to optimizing the overall devices’ processability, performance, and lifetime. These properties can be measured simultaneously utilizing the HR 30 rheometer’s parallel plate dielectric accessory. Insulating materials with a low dielectric constant (generally in the range of 1–5) are critical in electronic devices to prevent short circuits, protect signal reliability between components, and maintain device reliability [14,15]. To assess the insulating properties, κ can be calculated with the simple relation in Equation 2. Where ε₀ is the permittivity of free space (8.854 pF/m). The κ ranges from 2.1 to 5.9 for the PCM TIM, 2.4 to 3.3 for the BNS TIM, and the SF TMM has a constant value of 1.5. These values are all within the desired range for electrical insulation.

Figure 4. Storage permittivity as a function of temperature is shown for the three materials
Figure 4. Storage permittivity as a function of temperature is shown for the three materials

Figure 4 shows the storage permittivity (ε′) as a function of temperature for the three materials. The BNS TIM and PCM TIM both exhibit an increasing ε′ with temperature. Along with this the PCM shows a much stronger temperature dependence compared to the BN filled silicone pad. In contrast, the SF TMM has a relatively lower and temperature independent ε′ with temperature. Along with this the PCM shows a much stronger temperature dependence compared to the BN filled silicone pad. In contrast, the SF TMM has a relatively lower and temperature independent ε′. To assess the insulating properties κ can be calculated with the simple relation in Equation 2.

Where ε0 is the permittivity of free space (8.854 pF/m). The κ ranges from 2.1 to 5.9 for the PCM TIM, 2.4 to 3.3 for the BNS TIM, and the SF TMM has a constant value of 1.5. These values are all within the desired range for electrical insulation.

Figure 5. a) ε′ versus DE frequency and b) DE loss tangent versus DE frequency
Figure 5. a) ε′ versus DE frequency and b) DE loss tangent versus DE frequency

Figures 5a and 5b show ε′ and the loss tangent versus frequency, respectively, for BNS, PCM, and SF at 40 °C. The results in 5a show the frequency dependence of the storage permittivity. PCM exhibits the highest permittivity, decreasing gradually from about 30 to 25.5 pF/m as frequency increases, indicating noticeable dielectric dispersion and the progressive loss of slow polarization mechanisms. BNS shows an intermediate and nearly frequency-independent value of approximately 24 pF/m, indicating good dielectric stability. SF has the lowest permittivity, with an initial decrease at low frequencies followed by a stable plateau near 13.5 pF/m. Overall, PCM provides the greatest dielectric storage capacity, whereas BNS displays the most stable response over the investigated frequency range. Figure 5b shows PCM has a greater dielectric loss tangent compared to BNS and the PCM has a decreasing trend with increasing frequency.

Figure 6 shows the temperature-dependent shear modulus of the three samples from the simultaneous rheo-dielectric measurement. The PCM TIM has an expected modulus decrease as the material is heated and goes through its phase transition. Within the temperature range tested, the two silicone-based materials were not expected to show any transitions except for slight softening. This is observed in the SF TMM, but the high ceramic loading in the BNS TIM contributes to most of the shear modulus.

Data Analysis

Figures 7a and 7b present a min-max normalization of the collected data at 40 and 80 °C plotted on parallel coordinates, respectively. The two temperatures chosen are the general temperature range for electronic devices. These plots allow quick comparison of the various materials and enable material selection for a desired application. They provide information on thermal conductivity, insulation properties, and mechanical strength all on one plot. Normalization makes the comparison of each property relative. However, this is required to prevent skewing the comparison by scale.

Figure 6. Shear rheology from simultaneous rheo-dielectric temperature ramp
Figure 6. Shear rheology from simultaneous rheo-dielectric temperature ramp
Figure 7. Min-max normalization to compare and choose appropriate TMM at a) 40 °C and b) 80 °C
Figure 7. Min-max normalization to compare and choose appropriate TMM at a) 40 °C and b) 80 °C

Conclusions

The need for efficient TMM materials has been necessitated due to advancements in electronics that include device miniaturization, higher power densities, and greater functional integration. Material development to meet these challenges requires robust methods to quickly compare the materials based upon properties to develop fit for purpose materials. In this note, two classically defined TIMs and a thermal runaway pad were tested for three defining parameters: thermal conductivity, insulating properties, and shear mechanical strength. A simple analysis was then presented to allow quick material comparison and therefore expediting the selection process.

The FOX 50 HFM was used in conjunction with the HR 30 Rheo-Dielectric accessory to obtain the thermal, electrical, and mechanical properties of the three materials as a function of temperature. The TIMs showed to have greater thermal conductivity compared with the SF TMM. The only material that showed a temperature dependence on its G′ was the PCM TIM, which was anticipated from the inherent transition the material is designed to have. Both TIMs showed an increase in storage permittivity with temperature while the SF TMM remained almost constant. The dielectric frequency sweeps showed PCM to provide the greatest dielectric storage capacity, whereas BNS displays the most stable response over the investigated frequency range. While relative permittivity alone cannot be used to assess the electrical insulating performance of a material, the combination of a low dielectric constant, electrical conductivity below the practical detection limit of the HR dielectric accessory, and low dielectric loss tangent provides consistent evidence of good insulating behavior. Plotting these properties on parallel coordinates with a min-max normalization provided an efficient way to compare the materials.

References

  1. K. Razeeb and E. Dalton, “Nexalus,” [Online]. Available: www.nexalus.com/wp-content/uploads/2026/02/Present-and-future-thermal-interface-materials-for-electronic-devices.pdf. [Accessed 12 05 2026].
  2. Grandview research, “Thermal Interface Materials Market Summary,” Grandview Research, San Francisco, 2024.
  3. Y. Cui, M. Li and Y. Hu, “Emerging interface materials for electronics thermal management: experiments, modeling, and new opportunities,” J. Mater. Chem. C., vol. 8, pp. 10568-10586, 2020.
  4. Z. Dou, C. Lei, K. Wu and G. Yu, “The development of thermal interface materials,” Nature Electronics, vol. 8, pp. 1146-1155, 2025.
  5. Y. Tu, B. Liu, G. Yao, H. Luo, X. Jia, J. Du and C. Xu, “A Review of Advanced Thermal Interface Materials with Oriented Structures for Electronic Devices,” Electronics, vol. 13, no. 21, p. 4287, 2024.
  6. Y. Ouyang, X. Li, H. Tian, L. Bai and F. Yuan, “A Novel Branched Al2O3/Silicon Rubber Composite with Improved Thermal Conductivity and Excellent Electrical Insulation Performance,” Nanomaterials, vol. 11, no. 10, p. doi.org/10.3390/nano11102654, 2021.
  7. M. Asif, S. Hussain and M. F. H. Iqbal, “Heat Transfer Studies with PCM as Thermal Interface Material,” in Emerging Trends in Mechanical and Industrial Engineering, Singapore, Springer, 2023, pp. 223-239.
  8. C. Zhao, Y. Li, C. Jiang, Y. Tang, Y. He, W. Yu and B. Cao, “Phase change thermal interface materials: From principles to applications and beyond,” Chin. Phys. B, vol. 34, p. 096301, 2025.
  9. J. Wynn, “Thermal Conductivity Testing – Heat Flow Meter Method vs. Xenon Flash Meter Method,” TA Instruments, New Castle DE, vol. TPP032.
  10. Y. Zhou, S. Wu, Y. Long, P. Zhu, F. Wu, F. Liu, V. Murugadoss, W. Winchester, A. Nautiyal, Z. Wang and Z. Guo, “Recent Advances in Thermal Interface Materials,” ES Materials & Manufacturing, vol. 7, pp. 4-24, 2020.
  11. G. Li, J. Zheng, Z. Cui and R. Guo, “Unusual temperature dependence of thermal conductivity due to phonon resonance scattering by point defects in cubic BN,” Phys. Rev. B, vol. 110, p. L060101, 2014.
  12. M. Staub and A. Janisse, “Properties of Phase Change Material (PCM) Thermal Pads: A Specialized Thermal Interface Material,” TA Instruments, New Castle DE, vol. TA501, 2026.
  13. A. Eletskii, “Phase Change Materials with Enhanced Thermal Conductivity and Heat Propagation in Them,” Physchem, vol. 2, no. 1, pp. 18-42, 2022.
  14. H. Yang, Y. Tuersun, P. Luo, Y. Chen, X. Huang, Q. Huang, X. Chen and S. Chu, “Electrically insulating thermal interface material with ultrahigh thermal conductivity enabled by vertical boron nitride fibers,” AIP Advances, vol. 14, p. 095301, 2024.
  15. M.-X. Nie, J. Wang, Q. Zhang, D. Han and Q. Fu, “Achieving low dielectric constant and high thermal conductivity polymer composites by using larger POSS functionalized boron nitride nanosheets,” J. Mater. Chem. A, vol. 12, pp. 24214-24225, 2024.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Mark Staub, PhD. The author would like to acknowledge Justin Wynn for his assistance in Thermal Conductivity experiments.

TA Instruments, Discovery, and SmartSwap are trademarks of Waters Corporation or its affiliates.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.