The Auto-Trim Accessory as a Tool to Prevent Oxidation in Polymer Melts

Keywords: Rheology, Oxidation, Auto-Trim

TB115

Abstract

Frequency sweeps are typical experiments when testing polymer melts rheology, as they provide a variety of information regarding the viscoelastic properties, as well as the complex viscosity, that can be on specific cases converted into dynamic viscosity via the Cox-Merz transformation [1]. However, some polymers are particularly prone to oxidation and degradation, which can affect the results obtained during rheological testing. A potential solution could be saturating the measuring chamber with nitrogen or another inert gas, but that might not be enough to prevent oxidation. In this technical brief, the TA Instruments™ Auto-Trim Accessory is demonstrated as a tool to limit oxidation in sensitive polymer melts.

Introduction

A typical rheological experiment on a polymer melt involves loading and trimming the sample at experimental temperatures. This requires opening the Environmental Testing Chamber (ETC) at least twice during the experiment preparation. When the ETC is opened, air enters the furnace, and the sample is temporarily exposed to oxygen at high temperature. Additionally, it is difficult for the operator to be consistent with time to load and trim the sample, so across different experiments the sample might be exposed for different amounts of time.

The Auto-Trim Accessory (Figure 1) provides the advantage of being able to perform the trimming procedure automatically, eliminating the need to open the ETC [2]. The loading and experimental procedure changes to avoid the exposure of the sample to oxygen and high temperature at the same time.

Figure 1. The main components of the Auto-Trim Accessory
Figure 1. The main components of the Auto-Trim Accessory

Experimental

Low Density Polyethylene (LDPE) is a common polymer known for its oxidation instability. To show the benefits of the Auto-Trim, LPDE from Sigma Aldrich was tested.

Two different protocols were put in place, both performed at 160 °C with repetitions of frequency sweeps from 100 to 0.1 rad/s, 5 points per decade, 1% of strain. The geometry is a 25 mm parallel plate. In both protocols the ETC was flushed with nitrogen at 10 L/min at 2 bars.

The first protocol (Protocol One) is representative of a typical procedure when using the ETC. The ETC is pre-heated at 160 °C, then opened and the sample is loaded. The ETC is then closed, and the geometry is moved to trim gap (1.100 micron). After a short equilibration, the ETC is opened again, and the sample is trimmed manually. The ETC is then closed again, the geometry moved to experimental gap (1.000 micron) and when the normal force drops to approximately 0 N, the experiment begins. For this protocol, the LPDE sample is tested five times in a row, without removing the sample from the geometry, nor opening the furnace. A waiting time of 1 to 3 minutes is applied between subsequent sweeps. In total, approximately 25 minutes pass between the acquisition of the first and the last point.

A second protocol uses the Auto-Trim Accessory to perform the trimming process automatically. In Protocol Two, the ETC is cooled to a safe temperature below melting point (80 °C in this case), and the sample is loaded in the solid state. The ETC is then closed and left for 5 minutes to evacuate air completely. Temperature is then raised to 160 °C, and the geometry moved to the trim gap. The trim is performed automatically by the Auto-Trim Accessory, then the geometry is moved to experimental gap and the sweeps begin. In total, four sweeps were applied per sample, and three different samples were tested. Approximately 20 minutes pass between the acquisition of the first and the last point.

With the lambda function, the function is essentially defined in the script block in which it is being used, so in this case, the numerical integration loop. This option is shown here. The initial setup for the import of the required libraries, set up the kinetic constants, define the isothermal temperatures of interest, and creation of the dataframe are the same as above.

TB114 Code 18

The code looks similar with the exception that the definition of the function is contained within the iteration loop.

The final plot is generated in the same way, and the resultant plot is shown in Figure 5.

TB114 Code 19
Figure 5. Isothermal conversion plot where reaction order equals 1.8047. Ordinary differential equation generated separate from the numerical iteration loop.
Figure 5. Isothermal conversion plot where reaction order equals 1.8047. Ordinary differential equation generated separate from the numerical iteration loop.

A visual comparison of the isothermal conversion plots from the two function approaches shows these to be calculating the same result.

Results and Discussion

Results of Protocol One are shown in Figure 2. It is clear that the sample is not stable over time because of the exposure to oxygen and high temperature during loading and trimming. A drop of more than 10% in complex viscosity can be observed between the first and the fifth sweep.

The second protocol shows much better stability. Figure 3 shows the overlay of 12 scans (three samples, four scans per sample) and the reproducibility is significantly better than the standard protocol results.

Figure 2. Five frequency sweeps on LDPE using Protocol One (standard, without the Auto-Trim Accessory)
Figure 2. Five frequency sweeps on LDPE using Protocol One (standard, without the Auto-Trim Accessory)
Figure 3. Twelve frequency sweeps on LDPE using the Protocol Two (with the Auto-Trim Accessory)
Figure 3. Twelve frequency sweeps on LDPE using the Protocol Two (with the Auto-Trim Accessory)

Comparing the results of Protocols One and Two (Figure 4) shows that there is a significant difference between them. Manual trimming is in general less accurate than automatic trimming, thus bringing to different absolute values in the moduli and complex viscosity values.

Figure 4. A comparison of 12 Frequency Sweeps with Protocol Two (blue lines) and 5 sweeps with Protocol One (red lines)
Figure 4. A comparison of 12 Frequency Sweeps with Protocol Two (blue lines) and 5 sweeps with Protocol One (red lines)

Conclusions

Testing an oxygen sensitive sample such as LDPE can be challenging, even in a nitrogen flushed closed environment. The possibility of working automatically without opening the ETC by exploiting the capabilities of the Auto-Trim Accessory proved to be an excellent solution for obtaining consistent, accurate and reproducible results.

References

  1. J. D. Ferry, Viscoelastic Properties of Polymers, 3rd Edition, Wiley, 1980.
  2. K. Dennis, “Polymer Melt Rheology Workflow Automation: Auto-Trim Accessory for Discovery Hybrid Rheometers,” [Online]. Available: https://www.tainstruments.com/pdf/literature/RH127.pdf.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Marco Coletti, applications scientist at TA Instruments.

TA Instruments is a trademark of Waters Corporation or its affiliates.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.