TGA and DSC Testing of Energetic Materials

Keywords: Energetic Materials, Propellants, STANAG, TGA, TGA-MS, Hi-Res TGA, Constant Reaction Rate Hi-Res, DSC, Kinetics

TA505

Abstract

Accurate thermal analysis of energetic materials is critical for predicting storage stability, transport safety, and operational performance. This work applies TGA, TGA‑MS, Hi‑Res TGA, and DSC to investigate the thermal behavior of a sample propellant to demonstrate thermal analysis of energetic materials. The method development presented is focused on minimizing hazards while maintaining data integrity, including optimization of sample weight and heating rate. The material shows multiple weight loss steps, which were further investigated with evolved gas analysis to identify decomposition byproducts. Exothermic peaks were analyzed on DSC using the Flynn‑Wall‑Ozawa method to determine kinetic parameters of the decomposition. The complimentary techniques of TGA and DSC provide a comprehensive understanding of decomposition mechanisms and demonstrate a workflow for safe, standards‑aligned energetic materials characterization.

Introduction

Energetic materials are a class of chemical compounds and formulations that store a large amount of chemical energy and are designed to release that energy rapidly under appropriate initiation. This broad category includes explosives, propellants, and pyrotechnics [1]. Each kind of energetic material has its own energy release mechanism distinguished by intended function; for example, detonation in explosives and controlled gas generation in propellants. The different energetic material types have further sub-classes with different expected performances informed by chemical formulation and material processing conditions. Characterization of the thermal behavior of energetics is fundamental in their development. A clear understanding of thermal properties influences predictions of storage stability, safety, ageing, and end‑use performance and reliability.

Smokeless gunpowder is a solid propellant used in firearms that produces predominantly gaseous combustion products and generates less smoke and residue than traditional black powder propellants. It is engineered to burn in a controlled, progressive manner to generate the gas pressure that propels a projectile. Modern smokeless propellants are typically nitrocellulosebased (single‑base) or based on a blend of nitrocellulose and nitroglycerin (double‑base) [2]. They are formulated with blends of stabilizers, plasticizers, and other additives to control stability and performance. These compositional differences affect decomposition chemistry, heat release, and ignition sensitivity. The physical form of the propellant also affects the end-use performance. Smokeless gunpowder can come as flakes, extruded grains, or spherical “ball” powders. Powder geometry affects surface area relative to bulk volume, controls burn rate, and heat transfer; which all informs the performance of the propellant in a projectile [3].

The North Atlantic Treaty Organization (NATO) has implemented a series of Standardization Agreements (STANAGs) that define common processes, procedures, terminology, and technical and military equipment standards for its member nations. This collection of organizational standards includes methods for characterizing energetic materials [4]. STANAG 4515 specifically addresses thermal analysis methods for energetic materials. It provides guidance on the use of thermogravimetric analysis (TGA) and differential scanning calorimetry (DSC) for characterizing explosives and propellants. In practice, STANAG 4515 outlines standards for documentation of experimental conditions, conservative safety practices appropriate to energetic samples, and the reporting of key metrics, such as onset temperatures, peak temperatures, and weight loss steps [5].

Thermal characterization of smokeless gunpowder is central to understanding its stability, safety, and performance across storage, transport, and operational lifetimes. TGA and DSC are foundational instruments for studying the thermal properties of these propellants [2]. TGA records weight changes as a function of temperature, time, and atmosphere, which can be used to study volatilization, decomposition steps, and residue formation. Coupling a TGA with a gas‑phase spectrographic technique such as mass spectrometry (TGA‑MS) enables simultaneous analysis of off‑gassed degradation byproducts and weight loss, providing deeper insight into decomposition pathways [6]. DSC measures heat flow of thermal transitions and chemical reactions. Heat flow can be endothermic, which is when heat is absorbed by the sample, or exothermic when heat is released. Propellants will exhibit an exothermic peak from which onset and peak temperatures and enthalpies can be used as indicators of stability and reactivity. Together, these complementary instruments form the basis for comparative stability assessments, kinetic modeling, and hazard evaluation.

Experimental

Standard TGA

A commercially available double-base ball‑type smokeless gunpowder (SGP) was used in this work to demonstrate thermal analysis of energetic materials. The product is a slow burning powder for target loads that can be used for shotshell as well as a wide range of handgun calibers.

TGA experiments were performed on a TA Instruments™ Discovery™ TGA 5500. The instrument was purged with nitrogen gas at a rate of 25 mL/min through the balance chamber and 25 mL/min through the furnace. Samples were loaded onto clean 100 μL platinum pans for all TGA experiments. Preliminary testing revealed that conversion was completed by 300 °C, so that was set as the upper temperature for all TGA experiments. Using individual pellets as samples is preferred to create heat transfer uniformity between samples and increase run-to-run consistency. An iterative process was used to determine sample mass and heating rate for safety.

Hi-Res TGA

The Discovery TGA 5500 (as well as the Discovery TGA 550) can run in Hi-Res Constant Reaction Rate mode. Hi-Res TGA is a technique in which heating rate is dynamically changed in response to sample weight loss rate. In this way the thermal profile applied to a sample is dictated by the sample itself rather than being predetermined. In Constant Reaction Rate mode, the TGA changes the heating rate (even to the point of cooling) to try and maintain a certain weight loss rate [7]. The target weight loss rate is set by the resolution number in the TRIOS™ Software method, for example: a resolution number of -3 will target a weight loss rate of 1.00 wt%/min and -4 will target 0.316 wt%/min. While the relation of the resolution numbers and the target weight loss rates are not intuitive, the list of values can be found in the Hi-Res Operators Guide included with the TRIOS Software. A Hi-Res Constant Reaction Rate experiment was performed on SGP with a maximum heating rate of 2 °C/min and resolution and sensitivity numbers of -4 and 1 respectively.

TGA-MS

TGA-MS analysis was performed by connecting a Thermostar™ Mass Spectrometer from Pfeiffer Vacuum GmbH. The Mass Spectrometer Interface Kit (which includes a heated adapter) can be used to directly equip the transfer line onto the IR furnace of the TGA 5500. A bargraph recipe was used to analyze the evolved gas from the TGA-MS experiment scanning between 1-100 AMU. A dwell time of 64 ms was used, resulting in a total scan time of 6.6 seconds for the whole range. Mass fragments were measured with the Secondary Electron Multiplier (SEM) enabled for added sensitivity. After loading the sample in the furnace, a preliminary 15-minute isotherm was applied prior to a linear heating rate of 10 °C/min to 300 °C. The MS data collection was triggered at the beginning of the thermal ramp by a signal sent from the TRIOS Software. To increase ion-current signals, small pellets were sufficiently spaced out on the TGA pan to increase overall sample weight. Fragments grouped too close behave similarly to larger single pellets in the TGA and spontaneously ignite. Three small fragments were spaced along the outer diameter of the 100 μL platinum TGA pan to allow for an initial sample weight of 774 μg for TGA-MS experiments.

DSC

The preliminary testing performed with the TGA informed the experimental conditions for testing in DSC. Single SGP pellets (350 μg ± 50 μg) were loaded into TZero™ Aluminum DSC pans. The pans were sealed with aluminum TZero Hermetic Lids; however, a small hole was manually pierced in each lid with a needle to allow for volatiles to escape to not pressurize the pan. Samples were ramped from 40 °C to 250 °C at 1, 2, 5, and 10 °C/min in a TA Instruments Discovery DSC 2500. All experiments were performed under a 50 mL/min nitrogen purge.

Further analysis of the decomposition kinetics can be performed on these DSC results directly in the TRIOS Software, with the Kinetics Analysis Suite add-on [8]. Running the SGP at several heating rates allows for the isoconversional analysis of the major exothermic peak temperature across multiple rates as described in ASTM E698, also referred to as the Flynn-Wall-Ozawa method (FWO) [9]. This yields activation energies and pre‑exponential factors, which can let you compare formulations, check for batch-to-batch consistency, and model long term stability.

Results and Discussion

Standard TGA

STANAG 4515 does not mandate a specific sample weight for TGA or DSC experiments. It requires that sample size be minimized for safety while still maintaining data quality [5]. To find an appropriate sample size for the SGP used in this work, a series of 10 °C/min heating rate TGA experiments were performed with individual pellets of increasing initial weight from 337 μg to 1163 μg. The data is presented in Figure 1. For the two samples below 400 μg, a complete thermal degradation profile can be analyzed through the end of the test. The samples with larger initial weights, however, show an abrupt drop in weight. These TGA profiles show a sharp upward spike followed by an immediate drop to near zero, indicating a sudden energetic ignition which shakes the pan and hangdown wire and throws the sample from the pan. A sudden shake of that nature could cause the observed spike, and the weight signal immediately dropping indicates the loss of the sample. Based on these results, TGA experiments in the remainder of this work were performed on individual SGP pellets with an initial sample weight of 350 μg ± 50 μg.

Figure 1. TGA profiles of SGP of increasing initial weight all ramped at 10 °C/min. Initial sample weight indicated in the legend.
Figure 1. TGA profiles of SGP of increasing initial weight all ramped at 10 °C/min. Initial sample weight indicated in the legend.

In addition to determining the appropriate sample weight for testing, the heating rate of the experiment must also be determined. Figure 2 shows TGA curves of the SGP when ramped at increasing rates from 1-50 °C/min. A smooth continuous weight loss profile is observed at ramp rates up to 10 °C/min. At the faster rates the sample is lost after sudden ignition. Analyzing the time and temperature where these events occur as a function of different variables, such as heating profile or sample form, may be further studied. This work aimed to study the SGP during controlled thermal decomposition, so linear heating rates of 1, 2, 5, and 10 °C/min were used.

Figure 2. TGA profiles of SGP thermally ramped at increasing rates
Figure 2. TGA profiles of SGP thermally ramped at increasing rates

TGA degradation profiles of sample weight 350 μg at rates of 1, 2, 5, and 10 °C/min are presented in Figure 3. The SGP shows two distinct weight loss events in each curve, with the onset temperatures of both events shifting to higher values as the heating rate increases, which is indicative of a kinetically controlled process. The lower temperature step may correspond to the loss of volatile additives and/or moisture, while the higher temperature step may represent the primary thermal decomposition of the energetic material. All the runs have an equivalent final residue of 13 – 15 wt%. This consistent char formation across these runs can provide a useful comparative endpoint for quality control or ageing studies.

Figure 3. Full degradation profile of SGP ramped at 1, 2, 5, and 10 °C/min. The onset temperature of each weight loss step is indicated.
Figure 3. Full degradation profile of SGP ramped at 1, 2, 5, and 10 °C/min. The onset temperature of each weight loss step is indicated.

Although the initial sample weights were small (<400 μg), the TGA curves are clean and reproducible. The high-resolution microbalance and stable baseline performance of the Discovery TGA enables the instrument to deliver high-quality thermogravimetric data with minimal sample, which is important for safety when working with energetic materials.

Hi-Res TGA

Hi-Res Constant Reaction Rate mode can be a useful technique when testing an energetic material like this SGP. A slower degradation rate may keep a sample which can auto-ignite under control during a full degradation. A single experimental run could be performed to measure the percent residue without the need to optimize the experimental ramp rate conditions.

Data from a Hi-Res Constant Reaction Rate experiment on the SGP is presented in Figure 4. The maximum heating rate was 2 °C/min and the resolution and sensitivity numbers were set to -4 and 1, respectively. Figure 4 shows the continuously changing heating rate (green line) and overall thermal profile (red line) which the instrument was able to deliver to achieve the high degree of linearity in weight loss over time in the Hi-Res experiment. A final residue of 13 wt% is measured, which is consistent with the results observed in the linear heating rate experiments.

Figure 4. Weight loss over time (blue) for SGP run in Hi-Res Constant Reaction Rate mode. Changes in temperature (red) and heating rate (green) during the experiment plotted over time.
Figure 4. Weight loss over time (blue) for SGP run in Hi-Res Constant Reaction Rate mode. Changes in temperature (red) and heating rate (green) during the experiment plotted over time.

TGA-MS

The gas evolved during the TGA-MS experiment is presented in Figure 5. The mass fragments corresponding to gases identified by MS, which rose above the baseline signal, are displayed. These evolved gas signals are plotted against temperature, alongside the concurrently recorded TGA data. The weight loss profile and weight loss derivative (shown in the black solid and dotted line, respectively) can be directly compared to the gas evolution temperature in the same experiment throughout thermal degradation.

The significant mass fragment signals that displayed changes during the TGA run are plotted. This includes the signals for 2 AMU (hydrogen, H2), 12 AMU (carbon, C), 18 AMU (water, H2O), 30 AMU (nitric oxide, NO), 32 AMU (oxygen, O2), and 44 AMU (carbon dioxide, CO2). The mass fragment signals for 1 AMU (hydrogen fragment) and 17 AMU (hydroxyl fragment) were also observed during the test, but they were omitted from the figure to limit cluttering because the shape of those curves mirrored those of 2 AMU and 18 AMU (respectively), as is commonly observed in TGA-MS.

Figure 5. Weight loss and weight loss derivative for SGP (black) plotted against the ion-current signals for the observed mass fragments that evolved during the experiment
Figure 5. Weight loss and weight loss derivative for SGP (black) plotted against the ion-current signals for the observed mass fragments that evolved during the experiment

The peak ion current signals for all observed mass fragments show good agreement with the weight loss derivative and all the signals have maximum intensity during the second weight loss event along with the peak rate of weight loss. There are three mass fragment signals that show an increase in intensity during the initial weight loss step. 18 AMU shows an increase that may represent surface moisture. In addition, 44 AMU (CO2) shows an upturn in signal which, along with water, could be representing pyrolysis of lower stability additives. Finally, 30 AMU is observed to increase in this lower temperature region, which may be nitric oxide due to the nitrocellulose and nitroglycerin the SGP. However, different structures can have the same mass to charge ratio in TGA-MS so further analysis would have to be performed to confirm if the mass fragment signal of 30 AMU represents nitric oxide. It’s possible this signal represents a hydrocarbon segment or formaldehyde byproduct.

DSC

Figure 6 shows DSC traces for the SGP run at 1, 2, 5, and 10 °C/min. All the curves show the same broad exothermic decomposition beginning above 160 °C with peak exotherm temperatures that shift from 184 °C, for the slowest rate, to 204 °C at the fastest rate. The peak temperature shift with heating rate is expected for a kinetic thermal event. The DSC curves also have a smaller, reproducible exothermic peak centered near 100 °C whose onset and peak temperatures do not change with heating rate.

The small, lower temperature peak is observed on all runs except for the 1 °C/min ramp. The small sample size and slow heating rate may make it so there is insufficient signal to rise above the baseline for that run. The consistency of the peaks in the lower temperature exotherms suggests that the transition may not be kinetic, which suggests that they may represent a thermodynamic transition such as a phase change. The TGA results of SGP tested at the same ramp rates (Figure 3) does show a 30 wt% weight loss event that spans from 80 °C to 150 °C The onset of that low temperature weight loss event increases with increasing ramp rates, suggesting that event is kinetic. Further analysis will need to be done to understand the nature of these low temperature exotherms.

Figure 6. DSC ramp of SGP at 1, 2, 5, and 10 °C/min. Inset shows small exotherms observed at 100 °C. Onset and peak temperatures of exothermic peaks indicated.
Figure 6. DSC ramp of SGP at 1, 2, 5, and 10 °C/min. Inset shows small exotherms observed at 100 °C. Onset and peak temperatures of exothermic peaks indicated.

The TRIOS Software generated Flynn-Wall-Ozawa isoconversional plot for the SGP is presented, along with the determined kinetic terms, in Figure 7. An R2 value of 0.9999 supports the internal consistency of the multi-rate data for the analyzed conversion window. An apparent activation energy of 198 kJ·mol-1 is calculated. This indicates that the propellant is relatively inert at normal storage temperatures and reaction rates are very slow at low temperatures, but the rate will increase with temperature. The high pre-exponential factor of 45.8151 implies a high frequency of successful reactive events once the activation barrier is overcome, so once the process is thermally activated it proceeds rapidly. The calculated 60-minute half-life temperature is 165 °C. The 60-minute half-life temperature is the temperature at which the fitted kinetic model predicts the conversion to reach 50% in one hour, and can be used to quickly compare relative stability of the SGP tested here against different formulations.

Figure 7. Flynn-Wall-Ozawa isoconversional plot for SGP
Figure 7. Flynn-Wall-Ozawa isoconversional plot for SGP

Conclusions

The thermal properties of a double‑base smokeless gunpowder were characterized using TGA, Hi‑Res TGA, TGA‑MS, and DSC. Optimized experimental conditions enabled safe and complete measurement of decomposition of the energetic material. The sample was observed to have two weight loss steps and consistent residue formation. A primary exothermic event was observed in DSC above 160 °C. Evolved gas analysis and kinetic modeling provided deeper insight into decomposition pathways and stability.

References

  1. A. Yadav and S. Dharavath, “Shaping the future of energetic materials: breakthroughs, barriers, and emerging frontiers,” Chemical Communications, vol. 61, no. 85, pp. 16547-16559, 2025.
  2. K. Rahim, A. Samsuri, S. Jamal, S. Nor, S. Rusly, H. Ariff and N. Latif, “Key attributes of nitrocellulose-based energetic materials and recent developments,” Heliyon, vol. 11, no. 1, 2025.
  3. S. A. J. T. Lysien K, “Solid Propellant Formulations: A Review of Recent Progress and Utilized Components,” Materials, vol. 14, no. 21, p. 6657, 2021.
  4. W. P. De Klerk, “Thermal Analysis of Some Propellants and Explosives with DSC and TG/DTA,” 1996.
  5. NATO, EXPLOSIVES. THERMAL ANALYSIS USING DIFFERENTIAL THERMAL ANALYSIS (DTA). DIFFERENTIAL SCANNING CALORIMETRY (DSC), HEAT FLOW CALORIMETRY (HFC), AND THERMOGRAVIMETRIC ANALYSIS (TGA), Brussels, Belgium, 2015.
  6. TA Instruments, “TA495 Thermal Degradation and Evolved Gas Analysis of Lithium-Ion Battery Cathode Materials at Different States of Charge,” [Online]. Available: https://www.tainstruments.com/pdf/literature/TA495.pdf.
  7. TA Instruments, “TA075 DECOMPOSITION KINETICS USING TGA,” [Online]. Available: https://www.tainstruments.com/pdf/literature/TA075.pdf.
  8. TA Instruments, “TA073 A Review of DSC Kinetics Methods,” [Online]. Available: https://www.tainstruments.com/pdf/literature/TA073.pdf.
  9. ASTM International, ASTM E698-23: Standard Test Method for Kinetic Parameters for Thermally Unstable Materials Using Differential Scanning Calorimetry and the Flynn–Wall–Ozawa Method, 2023.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Andrew Janisse, Ph.D.

TA Instruments, Discovery, TZero, and TRIOS are trademarks of Waters Corporation or its affiliates. ThermoStar is a trademark of Pfeiffer Vacuum GmbH.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.