Shear Rate Calculations in Polymer Manufacturing Processes

Keywords: shear rate, rheology, extrusion, molding, polymer processing

TB118

Abstract

The shear rate of a polymer impacts its processability. The rate can vary throughout the stages of processing; for example, the shear rate may be one value in a molding cavity, and another as it enters the cavity. There isn’t a single shear rate for an entire machine so the engineer must consider this in process design. This note outlines the different shear rates experienced in various parts of polymer processes, such as extrusion and molding.

Introduction

Shear rate is the rate of deformation of a material and indicates how quickly the material is sheared, or worked, during flow. The shear rate may impact the material’s viscosity, which has important implications in the final application or processing of the material.

In simple shear, the shear rate, Ẏ, is the velocity gradient normal to the flow direction, Ẏ=dv/dy. In polymer processing, however, the engineer almost never calculates a full three-dimensional gradient field by hand. Instead, the usual practice is to identify the local flow geometry that controls the deformation, convert the production rate into a local volumetric flow rate Q, and then estimate a wall shear rate or an apparent wall shear rate from an idealized channel: circular, slit, annular, screw channel, or squeeze gap [1–3].

That point is crucial: there is no single shear rate for an entire machine. A polymer melt experiences different deformation histories in different regions. In injection molding, the gate may run at very high shear rate while the cavity itself is much lower. In extrusion, the metering section of the screw is governed by drag and pressure flow, whereas the die land is usually treated as Poiseuille-type flow. In blow molding, the die-head flow is primarily shear-dominated, but the subsequent inflation of the parison is mainly extensional. In compression molding, the relevant kinematics are often squeeze-flow rather than simple shear [4–9].

This note walks through various common polymer processing equipment and presents the applicable shear rate equations. Processes covered include injection molding, extrusion, blow molding, and compression molding.

Common Core Formulas

Circular channels: runners, nozzles, round gates, strand dies, capillaries

For a circular channel of radius R or diameter D, the standard apparent wall shear rate is

This is the Newtonian-equivalent wall value inferred from the volumetric throughput. For a shear-thinning polymer melt, the true wall shear rate is higher and is obtained through the classical Rabinowitsch-type correction. If the melt can locally be represented by a power-law index n, then

The engineering meaning is simple: once the velocity profile becomes flatter than the Newtonian parabola, the real wall gradient exceeds the apparent one [1,3].

Wide slit or thin rectangular channels: sheet dies, rectangular gates, thin cavities

For a slit of width W and thickness H, with W >> H, the apparent wall shear rate is

and, for a power-law melt,

This is the standard expression used when the flow is essentially one-dimensional across the thickness and side-wall effects are secondary. In polymer processing, this is one of the most important formulas because many real flows are locally well approximated by a slit: flat dies, micro-slits, thin-wall cavities, and many gate geometries [2–4].

Thin annular channels: tubing, pipe dies, blown-film dies, parison dies

For an annulus with outer diameter Do and inner diameter Di, a standard approximation is to “unwrap” the annulus into an equivalent slit whose width is the mean circumference and whose thickness is the annular gap. That gives

when the annular gap is small relative to the mean diameter. This approximation is widely useful in extrusion blow molding and tubing extrusion because the die land region is annular even though the downstream parison deformation is not [2,7].

Single-screw metering section

In the melt-conveying region of a single-screw extruder, the flow is classically decomposed into a drag-flow contribution caused by screw/barrel motion and a pressure-flow contribution opposed by die back-pressure. In flat-plate form, the throughput is represented as the superposition of those two terms, and the first-order estimate of the shear rate associated with drag is

where H is the channel depth and Vbz is the barrel velocity component in the down-channel direction. With barrel diameter D and screw speed N in rpm, the barrel surface speed is commonly written as V=πDN/60, and then projected along the channel helix if needed [5,6].

Compression or squeeze flow

In compression molding, a large part of the material motion is better described as squeeze flow between approaching surfaces than as developed channel flow. A useful average estimate is

where v is the closing speed, r is the characteristic flow radius, and h is the instantaneous gap. This is not a uniform local wall shear rate; it is an average kinematic measure for a radially spreading squeeze flow field [9].

Injection Molding

Injection molding must be decomposed region by region. The melt is plasticized by the screw, transferred through the nozzle, then passes through sprue, runners, gates, and finally the cavity. The local cross-section changes strongly along this path, so the local shear rate changes strongly as well. In practice, the most severe shear usually occurs where the flow area is smallest, very often at the gate, while the cavity experiences lower values once the flow fans out [4].

For a round runner or sprue of diameter D,

For a rectangular gate of width w and thickness h,

For a round gate of diameter d,

The important detail is that Q must be the local flow rate through that runner branch or that gate, not the machine output as a whole. If a runner splits into two equal branches, each branch carries roughly half the upstream flow. If a cavity is fed through multiple identical gates, the gate flow must be partitioned accordingly. That branching correction is often overlooked and creates major errors in shear-rate estimates [1–4].

A practical example shows the scale difference clearly. Suppose a cavity volume is 40 cm3 and the fill time is 1.0 s. Then

Q=40 cm3/s=0.00004 m3/s.

If the runner diameter is 5 mm,

If the gate is rectangular with w = 6 mm and h = 1.2 mm,

So, the gate shear rate is already almost one order of magnitude above the runner value. If the local power-law index is n = 0.4, then

This is exactly why gate sizing has such a strong influence on viscous heating, polymer degradation, gate blush, orientation, and filling pressure [2–4].

Inside a thin cavity, the local flow can often be approximated as slit flow. If the cavity thickness is hc and the local effective flow width is b(x), then

This is especially useful in thin-wall or micro-injection molding, where rectangular-slit approximations are widely used and where viscous dissipation can be strong enough to modify the local temperature field and therefore the apparent rheology during filling [4].

Extrusion

Single-screw extrusion: metering section

The metering section is not pure pressure-driven flow. It is a combined Couette-Poiseuille system. Screw rotation drags the melt forward, while die resistance generates a pressure gradient that drives backflow. That is why screw design, channel depth, viscosity, and die pressure are tightly coupled in the actual throughput [5,6].

Take an example with barrel diameter D = 60 mm, screw speed N = 100 rpm, helix angle ⌀ =17°, and channel depth H = 5 mm. The barrel speed is

The down-channel component is

So, the nominal drag-related shear rate is

That is a reasonable order-of-magnitude estimate for the metering channel itself. It is usually much lower than the shear rate in a restrictive die-land or a very small adapter [5,6].

Circular extrusion dies

For strand dies, pelletizing dies, and other circular outlets, use the circular formula. Suppose the line produces 20 kg/h of melt with melt density 760 kg/m3 through ten equal holes of diameter 3 mm. Each hole carries

and therefore

This is a typical moderate die land shear rate for many strand-type operations [1,3].

Slit dies

For sheet and cast-film dies, use the slit expression

Suppose W = 1.0 m, H = 1.0 mm, output 120 kg/h, and melt density 740 kg/m3. Then

and

That order of magnitude is entirely typical for wide flat dies unless the gap is reduced sharply or the throughput is pushed much higher [2,3].

Annular dies

For tubing, pipe, blown film, and extrusion blow-molding parison dies, use the annular approximation. If Do = 30 mm, Di = 26 mm, output 50 kg/h, and melt density 760 kg/m3,

and

That is the relevant die land shear rate during parison formation, not during the later free-hanging or inflation stage [2,7].

Blow Molding

Blow molding must be split into two very different deformation stages. Inside the annular die head and die land, the melt is still in a confined shear flow, so the annular shear-rate formula is appropriate. Once the parison leaves the die, hangs under gravity, and then inflates, the deformation is no longer best described as simple shear. At that point the dominant kinematics are extensional, often biaxial in stretch-blow applications [7,8].

In extrusion blow molding, parison geometry is controlled by swell, sag, die geometry, and operating conditions. In stretch blow molding, the material is intentionally driven into high biaxial deformation states, so strain rate and extensional response become more informative than a single scalar shear rate. Therefore, when one asks for “the shear rate in blow molding,” the correct engineering answer is: in the die head, yes; during inflation, not really — the relevant quantity is primarily extensional deformation rate [7,8].

Compression Molding

Compression molding is often discussed too loosely in terms of “flow,” but the flow kinematics differ markedly from injection or extrusion. When a heated charge is squeezed between approaching platens, the polymer spreads radially. The deformation field is therefore closer to squeeze flow than to developed shear flow in a channel [9].

Using the average squeeze-flow estimate,

consider a case with r = 80 mm, h = 3 mm, and v = 4 mm/s. Then

This value is far below the gate shear rates typical of injection molding. It is also only an average descriptor, because the actual flow field varies with radius and with time as the gap closes [9].

Practical Calculation Sequence

In real process work, the safest sequence is always the same. First, choose the location of interest: runner, gate, cavity, screw channel, die land, annular gap, or squeeze gap. Second, convert mass rate to volumetric rate using melt density, not solid density. Third, use the local geometry to choose the correct formula. Fourth, apply a non-Newtonian correction if you need the true wall shear rate rather than the apparent one. Fifth, verify whether the local deformation is genuinely shear-dominated; if not, as in blowup or stretch-blow operations, switch to extensional measures instead [1–9].

Common Mistakes

A frequent mistake is to use total machine throughput everywhere instead of the local branch flow. Another is to use the wrong density when converting kg/h to m3/s. A third is to forget that most quick formulas give apparent wall shear rate, not true wall shear rate. A fourth is to apply a shear-rate concept to a stage that is primarily extensional. A fifth is to ignore wall slip, even though the standard formulas assume no-slip at the wall and Mooney-type considerations show that slip can change the interpretation of capillary-derived flow data substantially [1–3,7–9].

Conclusions

This note describes the shear rate calculations applicable for polymer molding and extrusion. It also discusses frequent mistakes and errors commonly made when designing processes with regards to shear rate.

References

  1. Mooney, M. “Explicit Formulas for Slip and Fluidity.” Journal of Rheology, 2(2), 210–222 (1931). doi: 10.1122/1.2116364.
  2. Laun, H. M. “Polymer Melt Rheology with a Slit Die.” Rheologica Acta, 22, 171–185 (1983). doi: 10.1007/BF01332370.
  3. Moon, D., Bur, A. J., Migler, K. B. “Multi-sample Micro-slit Rheometry.” Journal of Rheology, 52(5), 1131–1142 (2008). doi: 10.1122/1.2955511.
  4. Wu, W., Zhao, B., Mo, F., Li, B., Jiang, B. “In-line Steady Shear Flow Characteristics of Polymer Melt in Rectangular Slit Cavities During Thin-wall/Micro Injection Molding.” Materials & Design, 223, 111266 (2022). doi: 10.1016/j.matdes.2022.111266.
  5. Marschik, C., Roland, W., Osswald, T. A. “Melt Conveying in Single-Screw Extruders: Modeling and Simulation.” Polymers, 14(5), 875 (2022). doi: 10.3390/polym14050875.
  6. Béreaux, Y., Charmeau, J.-Y., Moguedet, M. “A Simple Model of Throughput and Pressure Development for Single Screw.” Journal of Materials Processing Technology, 209(1), 611–618 (2009). doi: 10.1016/j.jmatprotec.2008.02.070.
  7. Yousefi, A.-M., Collins, P., Chang, S., DiRaddo, R. W. “A Comprehensive Experimental Study and Numerical Modeling of Parison Formation in Extrusion Blow Molding.” Polymer Engineering & Science 47(1), 1–13 (2007). doi: 10.1002/pen.20662.
  8. Menary, G. H., Tan, C. W., Harkin-Jones, E. M. A., Armstrong, C. G., Martin, P. J. “Biaxial Deformation and Experimental Study of PET at Conditions Applicable to Stretch Blow Molding.” Polymer Engineering & Science, 52(3), 671–688 (2012). doi: 10.1002/pen.22134.
  9. Zhang, W., Silvi, N., Vlachopoulos, J. “Modelling and Experiments of Squeezing Flow of Polymer Melts.” International Polymer Processing, 10(2), 155–164 (1995). doi: 10.3139/217.950155.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Carlos Gracia, Ph.D., Principal Applications Scientist.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.