Pulse Mode UV LED Curing of an Oxygen-Sensitive Adhesive

Keywords: UV, Ultraviolet, Multi UV, Adhesive, Oxygen Inhibition

RH176

Abstract

The Waters TA Instruments™ Multi LED Photocure Accessory for Discovery™ HR Rheometers allows for continuous or pulsed excitation of four wavelengths of UV light (365, 385, 395, 405 nm), simultaneously or sequentially. This note will demonstrate the utility of pulsing a single wavelength (385 nm) on a commercial urethane acrylate adhesive to investigate the impact of oxygen exposure on the kinetics of the reaction.

Introduction

When ultraviolet (UV) light irradiates materials such as the adhesive studied here, initiators absorb the light to produce free radicals in the material. These radicals crosslink acrylic groups on the monomer/resin and propagate, continuing the reaction. The crosslinking does not consume the radical, so the reaction continues until one of 3 things occurs: a radical meets an inhibitor – a molecule that reacts but does not produce a reactive radical, two radicals react with each other to create a stable bond, or no more reactive acrylic groups remain. Oxygen is known to inhibit the crosslinking for acrylic based systems [1].

Rheology is used to monitor the crosslinking reaction [2]. The modulus of a material that crosslinks increases as the reaction progresses. The material cures from a low modulus liquid or gel to a high final modulus that is taken as the long-time plateau after irradiation. The initial modulus can be very low– in this work less than 1 kPa– and cure to a very stiff material with nearly 100 MPa – a 5 order of magnitude increase.

The Multi LED Photocure Accessory allows for irradiation with 4 different wavelengths (365, 385, 395, 405 nm) at variable power in multiple modes and combinations. This work will utilize the pulse mode to investigate the effects of oxygen inhibition of the UV curing reaction in a commercial UV curing adhesive.

Experimental

The adhesive used was a commercial urethane acrylate system. The HR-30 with the Multi LED Photocure Accessory was used in this work. A disposable acrylic lower plate (20 mm) and disposable aluminum upper plate (8 mm) were used with 0.5 mm starting gap. Ambient temperature was used. A TRIOS™ Software Conditioning-Options step with axial force control set to maintain 0± 0.1 N was programmed to prevent axial force buildup and monitor material shrinkage (step 1, not shown). An Oscillation Fast Sampling step was programmed with a target strain of 0.1 % amplitude and 1 μNm minimum torque.

The Multi-Wavelength UV conditioning step shown in Figure 1 was used for adhesive tested in air (Figure 2). This step pulsed 385 nm light 4 times starting 30 seconds into the oscillation measurement with 1 minute between the start of each pulse. An additional set of tests were conducted with a nitrogen purged sample and air exposed sample (Figure 3) using 598 s off time giving 10 minutes between the start of each pulse. After 1 hour, a 60 second illumination was used to fully cure the system.

Figure 1. TRIOS Software setup for illumination and sampling. A conditioning step to move the stage to maintain 0 axial force was also used.
Figure 1. TRIOS Software setup for illumination and sampling. A conditioning step to move the stage to maintain 0 axial force was also used.
Figure 2. Complex modulus (blue), Gap (red), and UV calibrated irradiance (green) for the adhesive cured in air. Four two-second pulses of 20 mW/ cm2 385 nm UV light on the acrylic UV adhesive. Each pulse is 1 minute apart, and the first pulse starts after a 30 second wait. The first pulse causes an observable but small change in the modulus that plateaus and no change in the gap. The second pulse shows a significant increase in modulus and a decrease in gap over 1 minute but plateaus. The third and fourth pulses show much higher increases in modulus in which the curing reaction appears to propagate itself to a final modulus that is ~90% of a fully-cured system using continuous illumination.
Figure 2. Complex modulus (blue), Gap (red), and UV calibrated irradiance (green) for the adhesive cured in air. Four two-second pulses of 20 mW/ cm2 385 nm UV light on the acrylic UV adhesive. Each pulse is 1 minute apart, and the first pulse starts after a 30 second wait. The first pulse causes an observable but small change in the modulus that plateaus and no change in the gap. The second pulse shows a significant increase in modulus and a decrease in gap over 1 minute but plateaus. The third and fourth pulses show much higher increases in modulus in which the curing reaction appears to propagate itself to a final modulus that is ~90% of a fully-cured system using continuous illumination.
Figure 3. Complex modulus (solid lines) and irradiation power (dashed lines) for comparison of the adhesive irradiated in air (blue) and with nitrogen purged sample. The samples were both irradiated with four pulses of 385 nm light at 20 mW/cm2 for two seconds every 10 minutes (600 s) and a 60 second irradiation at 1h (3600 s) to fully cure the sample. Both samples cured to a similar final modulus of 95.8 MPa and 95.0 MPa at 4000 s for the air and purged measurement, respectively.
Figure 3. Complex modulus (solid lines) and irradiation power (dashed lines) for comparison of the adhesive irradiated in air (blue) and with nitrogen purged sample. The samples were both irradiated with four pulses of 385 nm light at 20 mW/cm2 for two seconds every 10 minutes (600 s) and a 60 second irradiation at 1h (3600 s) to fully cure the sample. Both samples cured to a similar final modulus of 95.8 MPa and 95.0 MPa at 4000 s for the air and purged measurement, respectively.

Results and Discussion

The first experiment shown in Figure 2 shows the complex modulus, gap, and irradiation power over a 400 s measurement. The complex modulus reflects the reaction progression as the material hardens due to crosslinking. The gap decrease indicates shrinkage as the reaction progresses but is not as sensitive as the modulus.

The first pulse at 30 s indicates the impact of oxygen inhibition in the crosslinking reaction for this adhesive. Reactive radicals are created and begin crosslinking but the modulus plateaus and the reaction stalls. Another pulse at 90 s begins the reaction again but the reaction again plateaus after a significant increase in modulus indicating that some of the oxygen in the system has been consumed.

The stalled reaction is due to the presence of oxygen or other inhibitors of the reaction. After the first pulse, some of the oxygen has been used up to inhibit the reaction so the second pulse progresses the reaction further and sustains longer. The third and fourth pulses cause the reaction to continue on its own and the reaction rate reduces due to the lack of acrylic groups to react with. After four pulses, the material cures to within 10 % of the final modulus of a system that was cured with continuous illumination.

A nitrogen purge was implemented to test the hypothesis that oxygen inhibition was the reason that the modulus plateaus after the first UV pulse. Figure 3 shows the nitrogen purged experiment with longer delays between pulses alongside another measurement in air with no purge. The nitrogen purged sample was purged for one hour before starting the experiment and the purge was maintained throughout the experiment. The delay between pulses was increased to 10 minutes to better observe the kinetic behavior. After four pulses and a total test time of 1 hour, a 60 s irradiation was used to fully cure the system. Both samples cured to a similar final modulus of 95.8 MPa and 95.0 MPa at 4000 s for the air and purged measurement, respectively.

The behavior after the first two pulses is shown in Figure 4 for air and Figure 5 for nitrogen with linear scaling of the modulus. As in the earlier experiment (Figure 2) the reaction in air with no purge plateaus after ~60 seconds to a value of around 2 kPa. The second pulse shows a more definitive plateau with a significant increase in modulus to almost 30 kPa.

Figure 4. Linear scale complex modulus (blue) for the first (top) and second (bottom) pulse of the adhesive sample measured in air without nitrogen purge. These data are the same as in Figure 3 with different scaling.
Figure 4. Linear scale complex modulus (blue) for the first (top) and second (bottom) pulse of the adhesive sample measured in air without nitrogen purge. These data are the same as in Figure 3 with different scaling.
Figure 5. Linear scale complex modulus (blue) for the first (top) and second (bottom) pulse of the adhesive sample measured in nitrogen purge before and during the measurement. These data are the same as in Figure 3 with different scaling. Irradiance power is shown in green.
Figure 5. Linear scale complex modulus (blue) for the first (top) and second (bottom) pulse of the adhesive sample measured in nitrogen purge before and during the measurement. These data are the same as in Figure 3 with different scaling. Irradiance power is shown in green.

The nitrogen-purged adhesive shows markedly different behavior with a nearly linear increase in modulus after the first pulse. Likely there is still some inhibition as the rate is significantly slower than the second pulse, but the linear behavior indicates no further consumption of the radicals that propagate the reaction. The concentration of acrylic groups early in the reaction is very high relative to the number of active radicals so practically no rate decrease is seen due to the consumption of the acrylic group reactant. No consumption of radicals and no significant reduction of reactants result in the linear behavior shown.

After the second pulse, the modulus increases significantly to 30,000 kPa, which is roughly a third of the final modulus. The loss of monomer, low concentration of inhibitors that were used up in the first pulse, and decreased mobility in the system are likely to be key factors in the behavior shown.

Even though the same number of initiators were likely activated (same pulse power) the reaction rate drastically increased at the start of the second pulse for the nitrogen-purged sample. Any oxygen left in the system after 1 hour of purge or other inhibitors were likely consumed in the first pulse so the initial rate increase in the second pulse is much higher than the first pulse. The rate slows down because the reaction nears completion so there are significantly fewer acrylic groups to react with and the system stiffens, which may result in less reactivity. The reaction plateaus on the second pulse in the air exposed sample are due to the presence of inhibitors while, in nitrogen, the reaction plateaus are due to lack of reactants or potentially two radicals meeting.

The reaction for both the air-exposed and nitrogen-purged samples can be accelerated until the system is fully cured, which appears to be at a modulus of ~95 MPa. The third and fourth pulse progress the reaction further by creating a new set of previously inactivated initiators and the final 60 s illumination ensures that all productive initiators have created the maximum amount of reactive crosslinking sites as are available. Diffusion is limited as the material crosslinks and modulus increases so reactivity decreases.

Conclusions

The Multi LED Photocure Accessory was used to investigate the effect of oxygen exposure on the reaction kinetics of a commercial urethane acrylate adhesive. The pulsed excitation of 385 nm light initiated a reaction in an air-exposed sample that stalled after the initial pulses. The same system and irradiation conditions on a nitrogen-purged system resulted in a reaction that propagated until the lack of reactive sites and diffusion slowed the reaction. Subsequent exposure to continuous excitation for 60 s cured the system to a nearly identical modulus. The air-exposed system stalled due to oxygen consuming reactive radicals to produce unreactive radicals.

References

  1. C. Decker, A. Jenkins, Macromolecules, 1985, 1241
  2. Tianhong Chen “UV Curing Analysis Using A Rheometer” https://www.tainstruments.com/pdf/literature/RH032.pdf (accessed September 2nd, 2026)

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Kevin Whitcomb Ph.D, Applications Scientist at Waters Corporation.

Waters, TA Instruments, Discovery, and TRIOS are trademarks of Waters Corporation or its affiliates.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.