Keywords: Powder rheology, Dry electrode processing, Graphite, Polytetrafluoroethylene, Premixing
RH172
Abstract
Dry electrode processing has attracted increasing attention as an alternative to conventional slurry-based lithium-ion battery electrode manufacturing, offering potential reductions in cost, processing time, and environmental impact. However, it introduces additional challenges in powder handling, mixing, and coating, making the bulk properties of mixed powders important for process optimization. In this application note, the Waters TA Instruments™ Powder Rheology Accessory was used to characterize the powder shear and flowability properties of graphite-based anode powders composed of graphite, polytetrafluoroethylene (PTFE), and carbon black. The effects of PTFE binder content and pre-mixing intensity between the active material and conductive additive were investigated.
Powder cohesion, unconfined yield strength, flow function, and total flow energy were characterized to provide insight into formulation and mixing process design. Scanning Electron Microscopy (SEM) observations were used to relate the bulk powder properties to the underlying microstructure. The results show that increasing PTFE content and stronger pre-mixing influence interparticle binding, resulting in reduced flowability and increased flow energy.
The growing demand for lithium-ion batteries (LIBs) has increased the need for sustainable and cost-effective electrode manufacturing [1]. However, conventional slurry-based electrode fabrication requires large amounts of organic solvents, leading to high energy consumption during drying, solvent recovery issues, environmental and safety concerns, and the potential formation of defects in the electrode structure during solvent evaporation [2]. To address these limitations, solvent-free dry electrode processing has attracted significant attention as an alternative process. By eliminating the use of solvents and the subsequent drying step, it can reduce manufacturing time, energy consumption, and processing cost compared with conventional slurry-based routes [3]. However, because liquid solvents are not used in the dry process, the mechanical and rheological properties of the mixed powder itself become critical factors governing powder handling, coating behavior, and overall processability [4].
In dry electrode processing, the mixed powder is directly handled, transported, fed, compressed, and sheared during processing. Therefore, powder flowability strongly affects process continuity, feeding stability, and the uniform supply of materials during scale-up [4, 5]. In calendar-based dry electrode fabrication, the powder mixture undergoes mixing, kneading, binder fibrillation, and roll pressing or lamination onto the current collector, where it is subjected to compressive and shear stresses [5, 6]. Under these processing conditions, insufficient flowability can cause unstable feeding and non-uniform coating, whereas excessive cohesion or poor particle rearrangement can result in thickness variation, density inhomogeneity, and defects in the formed electrode layer [4, 6]. For this reason, quantitative evaluation of the powder rheological response under consolidation and shear conditions is essential for understanding the processability of dry electrode powders.
Graphite is the most widely used anode active material owing to its high theoretical capacity, stable cycling behavior, good electrical conductivity, natural abundance, and relatively low cost [1]. In graphite-based dry electrode systems, carbon black (CB) is commonly used as a conductive additive to form electron-conducting pathways, while polytetrafluoroethylene (PTFE) binder contributes to mechanical integrity through shear-induced fibrillation during mixing and kneading [4, 7]. However, the relative contents of CB and PTFE can significantly influence the rheological properties of the mixed powder. Excessive CB content may deteriorate the internal cohesion and adhesion of the powder, whereas excessive PTFE content may reduce the continuity of conductive pathways and increase electrode resistance [4, 7]. Therefore, optimizing the composition and mixing conditions of graphite/CB/PTFE mixed powders is important for achieving stable powder handling, uniform dry electrode formation, and ultimately reliable electrode properties.
In this application note, the rheological properties of graphite-based mixed powders composed of active material, conductive additive, and binder are analyzed with respect to powder composition and pre-mixing conditions. Powder rheology measurements were conducted using the Powder Rheology Accessory on a TA Instruments rheometer. For more information about available rheology and rheometers, visit the TA Instruments product pages.
The mixed anode powder samples were composed of Gr (from Ito Graphite), CB (from MTI Korea), and PTFE (from MTI Korea). Five powder compositions were prepared with Gr:PTFE:CB weight ratios of 90:9:1, 90:7:3, 90:5:5, 90:3:7, and 90:1:9.
To investigate the effect of pre-mixing of the active material and conductive additive on the rheological properties of the mixed powder, Gr:PTFE:CB powder with a weight ratio of 90:5:5 was prepared under three different mixing conditions. In the first condition, Gr, CB, and PTFE were mixed directly using a HT-120 DX overhead stirrer (from DaiHan Scientific) at 400 rpm for 10 min. In the second condition, Gr and CB were first pre-mixed using an AR-100 planetary mixer (from Thinky) at 2000 rpm for 2 min, followed by the addition of PTFE and further mixing using the overhead stirrer at 400 rpm for 10 min. In the third condition, Gr and CB were pre-mixed using the planetary mixer at 1000 rpm for 2 min, followed by the addition of PTFE and overhead stirring at 400 rpm for 10 min.
Powder rheology tests were performed on a Waters TA Instruments Discovery™ HR 30 Rheometer using the Powder Rheology Accessory shear and flowability accessories, shown in Figure 1. The powder shear test was conducted according to ASTM D7891, with a 9 kPa pre-shear consolidating stress and subsequent shear steps at 7, 6, 5, 4, and 3 kPa consolidating stress.

Figure 1. Discovery HR 30 Rheometer (a) shown with the Powder Rheology Accessory shear cell (b) and flow cell (c).
The powder flowability test was conducted at a rotor tip speed of 60 mm/s. Data analysis was performed in TRIOS™ Software using the automated powder analysis software feature. Additional details on the powder rheology test and analysis procedures can be found in Waters TA Instruments application notes RH123 and RH125 [8, 9]. The particle size, shape, and surface morphology of the powder samples were investigated by SEM using a COXEM CX-200 SEM. The powder samples were prepared on double-sided carbon tape and imaged at a 20 kV accelerating voltage.
To correlate the microstructure with the rheological properties, scanning electron microscopy (SEM) was used. Figures 2a–e show SEM images of the mixed powders with PTFE contents ranging from 1 to 9 wt%. At low PTFE content, localized agglomerates in the powder are relatively small. As the PTFE content increases, larger localized agglomerates are observed. The mixed powders were Pt-coated and imaged at a 20 kV accelerating voltage.

Figure 2. Scanning electron microscopy (SEM) of 90:9:1 (a), 90:7:3 (b), 90:5:5 (c), 90:3:7 (d), and 90:1:9 (e) anode powders.
Figures 3a–c show SEM images of the mixed powders prepared with different pre-mixing conditions using a planetary centrifugal mixer. Without pre-mixing, localized agglomerates are observed in the Gr-based anode mixed powder, suggesting non-uniform distribution of the conductive additive within the active material matrix. As the pre-mixing intensity increases, the powder mixture shows a more uniform distribution, and the localized agglomerates become smaller.

Figure 3. Scanning electron microscopy (SEM) of anode powders without pre-mixing (a), with pre-mixing at 1000 RPM (b), and 2000 RPM (c).
Powder electrode processing includes feeding raw materials into processing equipment, mixing the powder, and dry coating the electrode under shear. Powder cohesion and flowability are critical for electrode powder processing. The powder should have good cohesive properties while maintaining adequate flow to allow efficient transport and mixing. The powder shear data for the five anode powder formulations and the powders prepared under different mixing conditions are shown in Figure 4.

Figure 4. Powder shear data after using locus analysis with Mohr circle construction of the five anode materials varying carbon black and PTFE content (a), and three anode materials varying mixing conditions (b).
Table 1 shows the shear properties obtained from the yield locus analysis performed in TRIOS Software. Cohesion, unconfined yield strength, and major principal stress increased with increasing PTFE binder content. As described in application note RH125 [9], the flow function can be determined by taking the ratio of major principal stress to unconfined yield strength and is used to classify powder flowability. Following the Jenike flowability classification system, all five powder formulations fall within the easy-flowing regime, which corresponds to a flow function between 4 and 10. However, the flow function gradually decreased with increasing PTFE binder content.
| Gr / PTFE / CB | Cohesion (kPa) | Unconfined Yield Strength (kPa) | Major Principal Stress (kPa) | Flow Function (-) |
|---|---|---|---|---|
| 90/1/9 | 0.45 | 1.58 | 15.28 | 9.68 |
| 90/3/7 | 0.46 | 1.64 | 15.36 | 9.42 |
| 90/5/5 | 0.49 | 1.75 | 15.30 | 8.51 |
| 90/7/3 | 0.51 | 1.79 | 15.22 | 8.62 |
| 90/9/1 | 0.64 | 2.21 | 15.06 | 8.76 |
The SEM images in Figure 2 help explain this trend, as the higher PTFE content is consistent with the formation of a more cohesive particle network. As a result, the powders with higher polymer content exhibit lower flow function and greater cohesion.
Table 2 shows the shear properties obtained from the yield locus analysis performed in TRIOS Software. The flow function decreased with increasing powder mixing intensity. Following the Jenike flowability classification system, all three powders fall within the easy-flowing regime, which corresponds to a flow function between 4 and 10. This suggests that stronger pre-mixing reduced the relative ease of powder flow, although the powders remained in the easy-flowing range.
| Samples | Cohesion (kPa) | Unconfined Yield Strength (kPa) | Major Principal Stress (kPa) | Flow Function (-) |
|---|---|---|---|---|
| Without re-mixing | 0.50 | 1.76 | 15.44 | 8.75 |
| Pre-mixing 1000 RPM | 0.52 | 1.82 | 15.13 | 8.29 |
| Pre-mixing 2000 RPM | 0.57 | 2.00 | 15.40 | 7.70 |
Powder flow tests provide insight into powder flowability and effective material transport for processing. Figure 5 shows the total flow energy under confined and unconfined conditions. Confined conditions occur when the impeller rotor moves downward, and unconfined conditions occur when the rotor moves upward. The samples with higher PTFE content show higher total flow energy in both cases, indicating that the addition of PTFE requires the rotor to do more work to move up and down through the powder bed. As shown in the SEM images (Figure 3) and shear results (Figure 4), PTFE fibrillation can promote agglomeration in the powder due to enhanced interparticle binding. This agglomeration leads to a higher energy input needed for sufficient flow.
Under confined measurement conditions, the total flow energy remains relatively stable during cycling. Localized polymer binder agglomerates can require the rotor to do more work to compress the powder as it moves downward during the confined flow step. In the unconfined measurement, particle binding increases the overall flow energy at higher PTFE content. However, because there is no compression step during the experiment, the total flow energy remains relatively steady throughout cycling.

Figure 5. Confined (a) and unconfined (b) flowability data for the Gr-based anode powder varying carbon black and PTFE content with a tip speed of 60 mm/s.
Figure 6 shows that the pre-mixed samples have higher total flow energy than the sample prepared without pre-mixing. The sample pre-mixed at 2000 rpm also shows higher flow energy than the sample pre-mixed at 1000 rpm. This indicates that pre-mixing increases the amount of work required for the rotor to move up and down through the powder bed. The further increase in flow energy at 2000 rpm suggests that stronger pre-mixing may enhance powder resistance to rotor movement, possibly due to increased particle binding or agglomeration during mixing.

Figure 6. Confined (a) and unconfined (b) flowability data for the Gr-based anode powder varying mixing condition with a tip speed of 60 mm/s.
As shown in the SEM images and shear results, pre-mixing improves the distribution of the conductive additive within the active material particles and reduces the size of localized agglomerates. However, pre-mixing can also promote the formation of cohesive particle networks. The particle binding and agglomeration may lead to a higher energy input needed for sufficient flow.
Under confined measurement conditions, the total flow energy shows a slight decrease as cycling progresses, even though repeated rotor motion can further mix the powder during the test. This suggests that the shear applied during the pre-mixing and main mixing steps was not sufficient to progressively form larger cohesive agglomerates during cycling. The presence of localized polymer binder agglomerates can still require the rotor to do more work to compress the powder as it moves downward during the confined flow step. In the unconfined measurement, the total flow energy remains relatively steady throughout cycling because no compression step is involved during the experiment.
In this study, graphite-based anode powders were analyzed to provide insight into optimizing electrode formulation and processing conditions. By utilizing the Powder Rheology Accessory, powder rheology characteristics of the mixed anode powder were systematically characterized, showing that flowability and flow energy were affected by increasing PTFE binder content. Pre-mixing of the active material and conductive additive also influenced the flowability and flow energy of the final mixed powder.
Higher PTFE content promotes PTFE fibrillation, which acts as a physical binder between anode powder particles and reduces powder flowability. Similarly, stronger pre-mixing improves the distribution of CB within the Gr particles but can also increase particle binding in the mixed powder. As a result, the powder shear analysis shows lower flow function and higher cohesion with increasing PTFE content and pre-mixing intensity. In the powder flow configuration with a smooth-surfaced cup and impeller rotor, this binding effect leads to higher total flow energy.
SEM image analysis confirmed that at higher PTFE contents, the fibrillation of the binder functions as a physical bridging agent between the anode particles, subsequently diminishing flowability. Accordingly, powder shear analysis indicates that as the PTFE content increases, the flow function decreases while cohesion increases. When evaluated under powder flow conditions utilizing a smooth-surfaced cup and impeller rotor, this interparticle binding effect results in an overall elevation of the total flow energy.
These results can be used to optimize powder formulation and mixing processes and to obtain more homogeneous anode powders that may contribute to reproducible and consistent electrochemical performance. Learn more about TA Instruments rheology and rheometers and powder characterization accessories.
References
- J. Li, J. Fleetwood, W. B. Hawley and W. Kays, “From Materials to Cell: State-of-the-Art and Prospective Technologies for Lithium-Ion Battery Electrode Processing,” Chemical Reviews, vol. 122, no. 1, pp. 903–956, 2021.
- A. Gyulai, W. Bauer and H. Ehrenberg, “Dry Electrode Manufacturing in a Calender: The Role of Powder Premixing for Electrode Quality and Electrochemical Performance,” ACS Applied Energy Materials, vol. VI, no. 10, p. 5122–5134, 2023.
- W. B. Hawley and J. Li, “Electrode Manufacturing for Lithium-Ion Batteries—Analysis of Current and Next Generation Processing,” Journal of Energy Storage, vol. 25, p. 100862, 2019.
- K. H. Lee, H. Shim, S. H. Lee, H. J. Kim, C. Park, J. Choi and G. Song, “Dual-fibrous PTFE Structure Enabling Uniform and Thick Dry Electrodes for High-Energy-Density and Long-Lasting Batteries,” Energy & Environmental Science, vol. 18, no. 18, pp. 8446–8461, 2025.
- E. Gwag and S. Y. Kim, “Flowability Evaluation for PVDF-Mediated Solvent-Free Li-Ion Battery Electrode Powders,” ACS Applied Energy Materials, vol. IX, no. 10, p. 6311–6318, 2026.
- Z. Gao, J. Fu, C. Podder, X. Gong, Y. Wang and H. Pan, “Particle Interactions during Dry Powder Mixing and Their Effect on Solvent-Free Manufactured Electrode Properties,” Journal of Energy Storage, vol. 83, p. 110605, 2024.
- M. Lux, C. Hänsel, A. Dupuy, C. Girsule, B. Schumm, S. Kaskel and C. Leyens, “Process-Property Relationships in Dry Powder Extrusion and Dry Electrode Coating of Lithium-Iron-Phosphate Cathodes,” Powder Technology, vol. 476, p. 122401, 2026.
- J. Vail, S. Cotts and T. Chen, “RH123: Powder Rheology of Lactose: Impacts of Powder Morphology on Performance of Pharmaceutical Excipients,” TA Instruments, New Castle, DE, United States.
- K. Dennis and S. Cotts, “RH125: Powder Rheology of Graphite: Characterization of Natural and Synthetic Graphite for Battery Anode Slurries,” TA Instruments, New Castle, DE, United States.
Acknowledgments
The authors thank Waters Corporation for providing valuable opportunities to participate in Academic Partnership Program.
For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.
This paper was written by Ye Jun Kim and Dr. Seon Yeop Jung from the Department of Chemical Engineering at Dankook University, Republic of Korea. Dr. Jung is currently with the Department of Chemical Engineering, Hongik University, Seoul, Republic of Korea.
TA Instruments, Discovery, and TRIOS are trademarks of Waters Corporation or its affiliates.