Multi-Wavelength UV Cure with Rheometer

Keywords: UV Curing, photopolymerization, multi-material additive manufacturing (MMAM), modulus, viscosity

RH173

Abstract

Complex polymer systems are useful in a variety of industrial applications due to their high spatial and temporal tunability [1]. In the field of multi-material additive manufacturing (MMAM), the ability to photocure materials at different wavelengths in a single vat significantly enhances both build efficiency and interlayer adhesion quality [2]. Furthermore, this curing method engenders precise spatial control of mechanical properties within the system. As single-vat MMAM becomes more commonplace in fields such as biomimetics and soft robotics, it is crucial that the mechanical properties of these material systems be characterized throughout the photocuring process. Photorheological analysis provides invaluable insight into how material and curing parameters (i.e., curing wavelength, irradiance, dosage) affect the strength and functionality of the overall system, helping researchers tailor a material system to their specific needs. In this study, the mechanical properties and kinetics of a dual-component epoxyacrylate system were characterized under 365 nm and 405 nm wavelengths using the Waters TA Instruments™ Multi LED Photocure Accessory.

Introduction

To illustrate the functionality of the UV-curing accessory, a dualmaterial photocurable system was analyzed. The system consisted of an acrylate oligomer that cures at 405 nm via photoinitiated free radical polymerization and an epoxy monomer that cures at 365 nm via photoacid-generated ring-opening polymerization. Due to kinetic differences, free radical polymerization induces curing in seconds, whereas ring-opening polymerization requires 30 seconds to several minutes of light exposure, followed by thermal post-curing. Prior research reports an optimal post-baking period of two hours [1].

A dual-component epoxy-acrylate system has a low-to-medium initial viscosity, depending on the component ratio and monomers used. This study utilized a 3:1 epoxy-acrylate system (by weight), which has an initial complex viscosity of around 4 to 6 Pa∙s. Photocuring results in the mechanical properties (G, G”, etc.) associated with this system to increase by several decades of magnitude. The acrylate is considered the “soft” component of this system, with a final G* in the kilopascal range (104 to 105 Pa), whereas the epoxy is considered the “stiff” component, with a final G* in the megapascal range (106 to 107 Pa).

This study examined the effects of UV light intensity on the mechanical properties of the single-component epoxy system, as well as the impact of multi-wavelength exposure and thermal postcuring on the curing conversion of the epoxy-acrylate system.

Multi LED Photocure Accessory

The Multi LED accessory provides the following wavelengths: 365 nm, 385 nm, 395 nm, and 405 nm. Each wavelength can be calibrated and activated using TRIOS™ Software to specify curing parameters such as wavelength and irradiance intensity/power (e.g., 5% for 365 nm or 10% for 405 nm), and exposure timescales (e.g., a 10-second pause with 20-second light exposure). The accessory was used to apply both 405 nm and 365 nm exposures in the same measurement, without the need to manually interchange external filters on a mercury lamp light source*.

* Mercury lamp measurements in this work were made using OmniCure™ S2000 UV Lamp

Figure 1. Multi LED Accessory and Upper Peltier Plate attached to HR rheometer
Figure 1. Multi LED Accessory and Upper Peltier Plate attached to HR rheometer

Experimental

Two photopolymerizable samples were analyzed via the UV-curing accessory on the Discovery HR Rheometer. The first of which was a single-component epoxy sample, while the second was a dual-material sample containing the epoxy and acrylate components in a 3:1 ratio by weight. The epoxy samples contained 2% (w/w) of a photoacid generator, and the acrylate samples contained 1% (w/w) of a photoinitiator, as these concentrations were considered optimal by the literature for multi-wavelength 3D printing [3,4].

The 365 nm and 405 nm wavelengths were calibrated via an external radiometer in this study. For all ambient tests, a 20 mm disposable acrylic plate was used as the bottom geometry, while thermal post-curing tests utilized a 20 mm quartz bottom plate. A 20 mm disposable aluminum plate was used as the top geometry for single-component testing, while an 8 mm disposable aluminum plate was used for the dual-component testing, including thermal post-baking. Oscillation fast sampling experiments were used to characterize the curing process. For all tests, the autostrain adjustment was programmed to maintain a strain rate of 0.01% to 100% and a torque of 4 μN∙m to 20,000 μN∙m. Fast data acquisition capabilities enabled the collection of two data points per second (1 Hz).

To determine the impact of UV intensity on curing, the epoxy sample was loaded onto the 20 mm acrylic plate with a 0.1 mm (100 μm) gap. The ideal gap geometry was determined by prior research on cycloaliphatic epoxides, such as the one used in this study [5]. An isothermal oscillation fast sampling test was performed at a frequency of 1 Hz and a strain of 0.1% with fast data sampling enabled. The 365 nm UV light was initiated 50 seconds after oscillation began, to establish an adequate baseline. The epoxy sample was tested at irradiances over the range of 10-100 mW/cm2, with an exposure time of 250 seconds for each test. The testing was conducted under ambient conditions (25°C).

To test the multi-wavelength capabilities of the LED accessory, the epoxy-acrylate system was loaded onto the 20 mm acrylic plate with a geometric gap of 0.1 mm (100 μm). An 8 mm aluminum upper plate was used as the top geometry. The 405 nm wavelength was initiated after 15 seconds, and the exposure time was set to 5 seconds for an irradiance of 2.5 mW/cm2 (Table 1). The 365 nm wavelength was initiated after 50 seconds, and the exposure time was set to 450 seconds at an irradiance of 10 mW/cm2. These standard photocuring parameters were selected based on literature results for similar dual cure 3D printable materials [2].

Table 1. Standard photocuring parameters for the epoxy-acrylate material system.

Wavelength (nm) Delay Time (sec) Exposure Time (sec) Irradiance (mW/cm2)
405 15 5 2.5
365 50 450 10

The epoxy-acrylate system was also tested with the mercury lamp accessory on the HR Rheometer, using the standard parameters (Table 1) to compare the light sources. A 400-500 nm bandpass filter was used to approximate the 405 nm wavelength, and a 365 nm bandpass filter was used for the 365 nm wavelength. However, the irradiance values were expressed in the program as a power level (%) to achieve greater wavelength accuracy. Prior to the test, the accessory was calibrated with both bandpass filters via an external radiometer. It was determined that the 405 nm exposure corresponded to a power output of 70.0%, while the 365 nm exposure corresponded to a power output of 16.0%, yielding the desired irradiance at each wavelength.

After the 400-500 nm wavelength was delivered to the sample, the filter was manually removed and replaced with the 365 nm filter during the 30-second period between the exposures. This test was conducted in ambient conditions (25° C).

As part of the thermal-post cure testing, the dual-component sample was loaded onto the 20 mm quartz plate with a 0.1 mm (100 μm) gap. Whereas the recommended temperature limit for the disposable acrylic bottom plate is 50°C, the quartz bottom geometry can be safely heated to 150°C. An 8 mm aluminum upper plate was used as the top geometry. The parameters outlined in Table 1 were utilized for the initial cure, and an additional oscillation fast sampling test was run immediately afterward with no light exposure. The thermal post-cure was initiated with an oscillation fast sampling test in which the temperature was ramped at 5°C/min from an initial temperature of 25°C to a final temperature of 50°C. This oscillation test was run for a total of 7,200 seconds following the temperature ramp at a strain of 0.1% and a frequency of 1.0 Hz, with the same auto-strain parameters as prior testing. The duration of the entire test (UV-cure and thermal post-cure) was 8,000 seconds, approximately two hours and 13 minutes.

To understand the effect of the thermal post-cure on the sample’s mechanical properties, control tests were performed using the LED UV-curing accessory and the Omnicure S2000 mercury lamp. Rather than heating the sample following the UV exposure period, these tests utilized an oscillation fast sampling step with a duration of 7,200 seconds at ambient temperature (25° C) (0.1% strain, 1 Hz frequency). Complex modulus data from the thermal and ambient test were analyzed at 5,000 seconds.

Results and Discussion

1. Influence of UV intensity on curing

Figure 2 illustrates the relationship between UV intensity and modulus (complex modulus, G*; storage modulus, G’; loss modulus, G”) for a single-component system. Although this study is primarily dedicated to the accessory’s multi-material curing capabilities, the single-component epoxy system was analyzed to establish a baseline change in modulus for a single material under different irradiances. Prior research has reported that the acrylate photoinitator absorbs in both the 365 nm and 405 nm range, and thus the modulus increase associated with the 365 nm exposure is not solely due to epoxy curing. Since quantitative characterization of the curing extent for each component at this wavelength lies outside the scope of this study, this initial single-component testing was utilized to gain insight into the epoxy’s curing behavior independent of the acrylate at 365 nm.

The intensity testing results indicated that the relationship between irradiance and mechanical properties such as complex modulus, G*, is not linear (Fig. 2). Whereas the conversion rate increases rapidly between the tests ran at 10 mW/cm2 (dark green) and 20 mW/cm2 (purple), the difference between the conversion rates for the tests ran at 50 mW/cm2 (light green) and 100 mW/cm2 (blue) is not significant. Figure 2 shows that 50 mW/cm2 is the point of diminishing returns for the epoxy component under these parameters. Thus, increasing the power beyond 50 mW/cm2 in this system would not significantly improve curing performance.

Figure 2. Complex modulus, G*, of the single-component epoxy system as a function of time for different irradiance values.
Figure 2. Complex modulus, G*, of the single-component epoxy system as a function of time for different irradiance values.

Gel point refers to the time at which a liquid sample transitions to a solid or gel and is represented by the crossover of the storage and loss moduli for a given sample (i.e., elastic, solid-like behavior predominates) [6]. This crossover point is visible for the curves associated with irradiances of 10 mW/cm2 and 50 mW/cm2 in Figure 3. For this material system, the gel point represents the beginning of curing. The conditions in Figure 3 were chosen to highlight the stark differences in gel point and curing characteristics due to irradiance. While the run at 10 mW/cm2 yielded a steady rate of conversion and a gel point of 190 seconds, the run at 50 mW/cm2 generated an immediate, high rate of conversion and a corresponding gel point of 35 seconds (Fig. 3). Although the storage moduli for both tests plateau at around 1 MPa, indicating maximum epoxy cure for the given parameters, the 50 mW/cm2 test is associated with an earlier plateau (especially evident from its loss modulus, G”).

Figure 4 provides an overview of the relationship between gel point and irradiance for all of the single-component epoxy intensity tests (Fig. 2). For the tests run at irradiance values of 50 mW/cm2 and greater, the gel point begins to plateau around 30 seconds (Fig. 3). This is further evidence of the diminishing returns regarding irradiance observed in Figure 2.

Figure 3. Storage modulus (green), G’, and loss modulus (blue), G”, as a function of time for the epoxy sample at 10 mW/cm2 (squares) and 50 mW/cm2 (triangles).

Figure 3. Storage modulus (green), G’, and loss modulus (blue), G”, as a function of time for the epoxy sample at 10 mW/cm2 (squares) and 50 mW/cm2 (triangles).

Figure 4. Gel point, t, as a function of irradiance for the single-component epoxy system.

Figure 4. Gel point, t, as a function of irradiance for the single-component epoxy system.

2. Multi-wavelength capabilities

Figure 5 illustrates the impact of light source on the complex modulus of the dual-component system at standard, ambient conditions (Table 1). The mercury lamp test yielded a much higher complex modulus—by nearly two decades of magnitude—as compared to the LED test. This suggests that the acrylate cured to a greater extent when exposed to the mercury lamp, but the use of bandpass filters must be considered. Whereas the LED source provides 405 nm of light at a high degree of accuracy (based on preliminary calibration testing), the mercury lamp utilizes a bandpass filter in the range of 400 to 500 nm. Thus, in the mercury lamp experiment, the photoinitiator that catalyzes the acrylate curing reaction is exposed to a much wider range of wavelengths, therefore leading to a greater cure extent. This also explains why the mercury lamp does not induce a greater cure than the LED light source at 365 nm, as the bandpass filter used was only for 365 nm. Although the mercury lamp cures the material slightly faster at 365 nm, as seen by the slope of the curve in Figure 5, the final moduli associated with the light sources are nearly identical (about 1.0 MPa).

While greater acrylate conversion at 405 nm may seem advantageous from an efficiency standpoint, bandpass filters are not representative of the additive manufacturing process for UV vat-polymerized materials. Given the sophistication of these material systems and their desired mechanical properties, it is crucial that exact wavelengths—rather than a 100-nm range—can be delivered to better replicate real-world processing conditions.

Figure 5. Complex modulus, G*, as a function of time for the epoxy-acrylate system, run with 405nm using the Multi LED accessory (blue) and the mercury lamp curing accessory with 400-500nm filter (green). Both runs utilized standard conditions (Table 1).
Figure 5. Complex modulus, G*, as a function of time for the epoxy-acrylate system, run with 405nm using the Multi LED accessory (blue) and the mercury lamp curing accessory with 400-500nm filter (green). Both runs utilized standard conditions (Table 1).

3. Influence of thermal post-cure on conversion

Figure 6 depicts the epoxy-acrylate system under thermal postcuring conditions. The slight decrease in G* immediately following the light exposure period is due to enhanced chain mobility associated with the increase in temperature (Fig. 6). However, G* begins to gradually increase around the 15-minute mark and continues to do so over the course of the two-hour heating period, consistent with heat-induced curing. From the end of the light exposure period (t = 500 seconds) to the end of the thermal post-cure (t = 8,000 seconds), the G* increases by a decade of magnitude, from 5.2 MPa to 55 MPa (Fig. 6).

Figure 6. Complex modulus, G*, as a function of time for the epoxy-acrylate system under thermal post-curing conditions (50°C). The center plot shows a magnified perspective of the post-curing run during the light exposure period (prior to heating). The thermal post-cure commences at the time indicated by the red line on the plot (500 seconds).
Figure 6. Complex modulus, G*, as a function of time for the epoxy-acrylate system under thermal post-curing conditions (50°C). The center plot shows a magnified perspective of the post-curing run during the light exposure period (prior to heating). The thermal post-cure commences at the time indicated by the red line on the plot (500 seconds).

At t = 5,000 seconds, the thermal post-cure test produced a complex modulus about three times higher than that of the LED and mercury lamp tests (Table 2). Since the thermally post-cured sample yielded a G* of 5.2 MPa at t = 500 seconds, the data in Table 2 suggests that this material system continues to cure in the absence of light or heat. However, a greater conversion rate is achieved when the sample is heated following the UV-cure.

Table 2. Complex moduli at 5,000 seconds for tests run with varying light sources and thermal conditions.

Light Source Temperature, T (°C) G* (MPa) at t = 5,000 sec
Mercury lamp (Omnicure S2000) 25 16.7
LED 25 14.5
LED 50 43.5

Conclusions

Using the Multi LED Photocure Accessory, this study analyzed several mechanical properties—G’, G”, and G*—associated with UV-curing of single- and multi-component material systems. Results indicated that the accessory can induce curing via 365 nm and 405 nm wavelengths, yielding mechanical properties consistent with the literature for an epoxy-acrylate material system [1]. Compared to light sources like mercury lamps, LEDs allow for more specific control of wavelengths, rather than a wide range of wavelengths via a bandpass filter (i.e., 400-500 nm). Lastly, the results illustrated the impact of thermal post-curing on the final modulus of the material system.

References

  1. Escriba-Flores, A. A., Fernández-Francos, X., Ferrando, F., & Fabregat-Sanjuan, A. (2025). Tunable dual-curing acrylic/epoxy systems for 3D printing with enhanced joint performance via carbon nanotubes. Polymer, 334, 128768. https://doi.org/10.1016/j.polymer.2025.128768
  2. Cazin, I., Gleirscher, M. O., Fleisch, M., Berer, M., Sangermano, M., & Schlögl, S. (2022). Spatially controlling the mechanical properties of 3D printed objects by dual-wavelength vat photopolymerization. Additive Manufacturing, 57, 102977. https://doi.org/10.1016/j.addma.2022.102977
  3. CPI-310B Ionic Photo Acid Generator, Photo-Cationic Polymerization Initiator (Sulfonium)—San Apro. (n.d.). Retrieved August 4, 2026, from https://www.san-apro.co.jp/en/products/acid-uv/cpi-310b/
  4. Yosef Tal, N., Dodiuk, H., Farran, S., Carmieli, R., Pinkas, I., Kenig, S., & Tenne, R. (2024). Accelerated Photocuring of Acrylate Resins with WS2 Nanoparticles. ACS Applied Polymer Materials, 6(6), 3303–3315. https://doi.org/10.1021/acsapm.3c03119
  5. UV intensity, temperature and dark-curing effects in cationic photo-polymerization of a cycloaliphatic epoxy resin. (2012). Polymer, 53(10), 2038–2048. https://doi.org/10.1016/j.polymer.2012.03.025
  6. Alemán, J. V., Chadwick, A. V., He, J., Hess, M., Horie, K., Jones, R. G., Kratochvíl, P., Meisel, I., Mita, I., Moad, G., Penczek, S., & Stepto, R. F. T. (2007). Definitions of terms relating to the structure and processing of sols, gels, networks, and inorganic-organic hybrid materials (IUPAC Recommendations 2007). Pure and Applied Chemistry, 79(10), 1801–1829. https://doi.org/10.1351/pac200779101801

Note

Any opinions, findings, and conclusions or recommendations expressed in this material are those of the author(s) and do not necessarily reflect the views of Rochester Institute of Technology.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

TA Instruments, Discovery, and TRIOS are trademarks of Waters Corporation and its affiliates.

OmniCure is a trademark of Excelitas Canada Inc.

This paper was written by Ryan T. Colburn, Alison Jackson, and Christopher L. Lewis, PhD., Advanced Polymers and Composites Laboratory, Rochester Institute of Technology, Rochester, NY USA

Click here to download the printable version of this application note.