Monitoring PDMS Through Edge Fracture on the ARES-G3 Rheometer Using Simultaneous Data Streams

Keywords: ARES-G3, Cone and Partitioned Plate, Dual Data, Harmonics, Edge Fracture

RH164

Abstract

The dual data feature on the ARES-G3™ Rheometer allows users to capture correlated and transient data in a single measurement. In this note, polydimethylsiloxane (PDMS) is monitored from the linear region through edge fracture using both streams of data. A more complete understanding of the material’s evolution using both data streams is presented.

Introduction

Simultaneous streams of correlated and transient data provide users with information-dense results in a single test. Transient data, or the time dependent stress and strain, is converted into correlated data using a Fourier transform. Correlated results provide instant feedback on material behavior and allow users to quickly compare samples or batches over time using material properties such as the viscous and elastic moduli and complex viscosity. Transient data may be correlated with user preferred methods or used to evaluate transitions from linear to nonlinear testing as well as the transition to edge fracture. While some material changes may be inferred from correlated data, the transformed data point does not tell the whole story. Transient data provides additional insights and methods for troubleshooting, especially for users interested in the nonlinear oscillatory behavior of materials. Nonlinear rheology has a rich history [1, 2] and is essential for quantifying material behavior during processing or end use conditions when materials experience large and/or rapid deformations. Nonlinear rheology has been applied to polymers [2, 3, 4, 5], adhesives [6], blood [7], chocolate [8], cheese [9], and gluten dough [10] to investigate end use conditions and microstructure.

Small Amplitude Oscillatory Shear (SAOS) measurements are some of the most common rheological experiments. SAOS measurements are performed within a material’s linear viscoelastic region [11] to determine the sinusoidal response to sinusoidal deformation. In this region, the moduli are independent of the applied deformation and the response is predictable. Increasing the deformation on a sample pushes the sample out of the linear region and into the nonlinear region.

Measurements outside of the linear region include medium and large amplitude oscillatory shear (MAOS and LAOS). The transition from linear to nonlinear measurements may be tracked through advanced analysis of the stress waves including Fourier analysis [4, 12, 13] and the Sequence of Physical Processes [14]. In this note, emphasis is given to evaluating odd harmonic contributions generated from Fourier analysis to establish boundaries from SAOS to MAOS to LAOS [1, 14, 15] while considering the impact of edge fracture [16].

LAOS data is often truncated prematurely due to edge fracture, which is the result of the second normal stress difference exceeding a material’s surface tension [3]. Edge fracture causes the effective sample diameter to be smaller, as illustrated in Figure 1, due to the expulsion of material from the gap when fracture occurs. TA Instruments™ Cone and Partitioned Plate Accessory (CPP), available on the ARES Platform, provides a solution to delaying the onset of edge fracture, which is prevalent for polymer solutions and melts [3]. As shown in Figure 2B, the upper geometry consists of a 10 mm parallel plate mounted on the transducer. The plate is coaxial with an outer 25 mm cylinder that is mounted to the stage. The accessory includes a lower 0.1 rad cone that is 25 mm in diameter and has an added lip to avoid sample dripping into the test chamber (Figure 2A). It is important to note that the CPP can be paired with any 25 mm diameter lower plate or cone. Cones are necessary for LAOS analysis because they provide a uniform shear profile and are used to achieve higher shear rates. However, parallel plates should be considered for samples that exhibit wall slip or have large particles. Parallel plates may be surface modified as crosshatched or serrated to address wall slip. Parallel plates are operated at larger gaps than the truncation gaps of cones, so samples with larger particles may be tested. The geometry, gap, and sample trimming also impact how edge fracture develops or propagates, so changing the geometry may aid in extending the measurement range.

The onset of edge fracture can be difficult to detect visually and through correlated data. Correlated data provides a summary of a material’s response to each deformation. Transient data shows each deformation cycle over time. The deformation is often requested for multiple cycles to improve averaging. To simplify data collection and gather rich data sets, simultaneous data streams may be collected on the ARES-G3 Rheometer. Having access to both data streams enables users to identify the exact data point where edge fracture begins impacting data quality, thereby improving confidence in measurement accuracy.

Figure 1. Illustration of effective diameter after edge fracture has occurred between parallel plates
Figure 1. Illustration of effective diameter after edge fracture has occurred between parallel plates
Figure 2. (A) Image of Cone and Partitioned Plate setup with sample loaded. (B) Upper CPP geometry showing mounting bracket, center plate shaft, and outer coaxial cylinder.
Figure 2. (A) Image of Cone and Partitioned Plate setup with sample loaded. (B) Upper CPP geometry showing mounting bracket, center plate shaft, and outer coaxial cylinder.

Experimental

Polydimethylsiloxane (PDMS) was tested at 30 °C with the Forced Convection Oven (FCO), providing fast-responding and uniform temperature control. Data was collected using the cone and partitioned plate geometries, including the 10 mm parallel plate and lower 0.1 rad cone with and without the partition installed. Oscillation-Amplitude tests at 10 Hz from 1–200% strain were performed with simultaneous data collection as shown in Figure 3A. The output of this simultaneous data collection example is shown in Figure 3B. Amplitude-1 includes the correlated results. Each Amplitude-1 [strain %] contains the transient data for the respective strain percentage. The correlated results include system corrections that are typical for these types of rheometer measurements. When frequency-based correlation is selected, the number of raw data collection cycles depends on the frequency. At 10 Hz, 120 half cycles are collected.

Additional analysis of the individual transient results is performed using the FT-Rheology or Fourier Transform Rheology package available as an add-on for TRIOS™ Software. This package allows for the analysis of transient oscillatory data to extract the fundamental and harmonic frequencies, which may be used to assess nonlinearity and edge fracture.

Testing revealed an anomaly for all samples at specific shear rates where the measured shear stress deviates from the expected monotonic increase. Instead of a smooth curve, the data exhibits erratic fluctuations in the stress response. This erratic stress response remains as an indirect indication of something being wrong, with rheological techniques alone not being able to definitively confirm any microstructural changes as a result of the applied shear.

Figure 3. (A) TRIOS Software procedure for amplitude strain sweep with simultaneous data collection. (B) TRIOS Software results output.
Figure 3. (A) TRIOS Software procedure for amplitude strain sweep with simultaneous data collection. (B) TRIOS Software results output.

Results and Discussion

Correlated Results and Point Display Data

A comparison of the correlated amplitude sweep data is shown in Figure 4. The data collected with the cone shows a decrease in the elastic (G’) and viscous (G’’) moduli at a lower strain percentage when compared to the CPP data. The decrease in oscillation torque during edge fracture occurs at a higher strain% for the CPP when compared to the cone as shown in Figure 4B. From 1 to 31.4%, both configurations agree well in terms of moduli and oscillation torque. The results for the cone begin to deviate from the CPP at 39.5%, indicating that the sample is impacted by edge fracture. In the absence of edge fracture, the oscillation torque would increase as strain increased. The design of the CPP delays the onset of edge fracture and allows users to collect additional data before the sample is destroyed by edge fracture.

One way to visualize the input stress and strain waveforms used for correlated data is through the Point Display. Here, a high level and reduced view of the waveforms may be used to assess the data quality or sample condition. Example Point Displays for CPP data are shown in Figure 5 for values in the linear region and where edge fracture has occurred. The linear region occurs at low strains where the moduli are parallel and independent of strain. Edge fracture is apparent in the high strain region where the moduli have decreased significantly along with the oscillation torque. In both the linear and edge fracture regions, the strain waves show sinusoidal behavior indicating that the mechanical deformation is high quality. At low strains, in the linear region of the sample, the stress responds to the deformation in a predictable, sinusoidal manner. At high strains, when the sample has undergone edge fracture, the stress wave is no longer sinusoidal and has an unpredictable response. The Point Display is useful for qualitative assessment; however, the data may not be used to calculate accurate material functions. The entire time-dependent evolution of the stress and strain waves is available with transient data collection. Transient data may be processed through TRIOS Software or with an external program to calculate material functions.

Figure 4. (A) Correlated amplitude sweep results for PDMS at 30 °C collected with a cone and the CPP. Results span the linear region (low strains) through edge fracture (high strains). (B) The corresponding oscillation torque for cone and CPP measurements.
Figure 4. (A) Correlated amplitude sweep results for PDMS at 30 °C collected with a cone and the CPP. Results span the linear region (low strains) through edge fracture (high strains). (B) The corresponding oscillation torque for cone and CPP measurements.
Figure 5. Point display examples from the linear and edge fracture regions for data collected with CPP
Figure 5. Point display examples from the linear and edge fracture regions for data collected with CPP

Transient Data and Harmonics

This simultaneous data measurement also includes the transient oscillatory data collected for each strain percentage. The data can be extracted and analyzed separately. The stress vs. strain or Lissajous plots corresponding to the same linear and edge fracture regions as in Figure 5 are shown in Figure 6. In the linear region, the Lissajous curve is elliptical, which is expected for viscoelastic materials [13]. Additionally, all 120 half cycles overlay well with each other. In the edge fracture region, the shape of the Lissajous curves deviate significantly from the elliptical shape and the half cycles do not overlay. As the sample edge fractures, the stress waves evolve. While the point display is an indication that the stress waves are impacted, the Lissajous plot provides a more accurate depiction of how the correlated data point is affected at a certain strain percentage. The time dependence of strain percentages ranging from 39.5 to 125 % is shown in Figure 7 for CPP measurements. Up to 78.9%, the difference in the stress peak of the first cycle and the stress peak of the last cycle is within 1%. At 99.3% and above, there is both apparent distortion and significant decrease in the stress waves with time because the sample is no longer intact. The onset of edge fracture likely occurs between 78.9 and 99.3% strain.

Figure 6. Lissajous plot examples, corresponding to Figure 5, for linear and edge fracture regions for data collected with CPP
Figure 6. Lissajous plot examples, corresponding to Figure 5, for linear and edge fracture regions for data collected with CPP

While changes in the shapes of stress curves and Lissajous plots are key indicators of the sample condition, more subtle changes such as the transition from linear to nonlinear regions may be quantified using FT-Rheology. To visualize the evolution of the harmonics, a 3-dimensional plot is shown in Figure 8 for 5–199% strain and the third, fifth, and seventh harmonics. In the linear region of the sample, these harmonics are not significant. As the sample transitions out of the linear region, the third harmonic becomes more significant. Harmonic ratios may be used to establish MAOS and LAOS regions [1, 14, 15]. When the ratio of the third harmonic to the first harmonic (I3/I1) exceeds 0.001, the data may be considered MAOS. When the ratio of the fifth harmonic to the third harmonic (I5/I3) exceeds 0.1, the data may be considered LAOS. In this example, I3/I1 > 0.001 starting at 19.8% strain and I5/I3 > 0.1 starting at 99.3% strain. It is noted that the LAOS region quantified by harmonics occurs near the edge fracture onset identified earlier where the transient stress wave decreased with time. Edge fracture is not a material property as it depends on the experimental setup and may vary between sample loads and geometries. It’s also noted that as the impact of edge fracture increases, the seventh harmonic contribution also increases.

Figure 7. Transient stress cycles over time from 39.5–125 strain% showing transition to edge fracture for data collected with CPP
Figure 7. Transient stress cycles over time from 39.5–125 strain% showing transition to edge fracture for data collected with CPP
Figure 8. Third, fifth, and seventh harmonics from 5-199 strain% for data collected with CPP
Figure 8. Third, fifth, and seventh harmonics from 5-199 strain% for data collected with CPP

Conclusions

In this note, PDMS was measured with a lower cone with and without a partitioned plate installed. The TA Instruments Cone and Partitioned Plate Accessory allowed for more data points to be collected because of the delay in edge fracture reaching the transducer. Simultaneous data streams on the ARES-G3™ Rheometer provided information-rich data sets with correlated and transient data. Having both data sets in a single measurement simplifies troubleshooting during and after test execution. The correlated points and Point Display provide a high-level view of the material’s response to an applied deformation. The transient data provides additional time dependent evolution of the material’s response. Both data streams may be utilized to troubleshoot or investigate materials undergoing the transition from linear to nonlinear oscillatory shear while considering the impact of edge fracture. Outside of the linear region, additional analyses are required to fully characterize and understand material behavior. The FT Rheology package available through TRIOS™ Software allows users to access nonlinear parameters, such as harmonics, to quantify the material response in this region.

References

  1. K. Hyun, M. Wilhelm, C. Klein, K. Cho, J. Nam, K. Ahn, S. Lee and R. M. G. Ewoldt, “A review of nonlinear oscillatory shear tests: Analysis and application of large amplitude oscillatory shear (LAOS),” Progress in Polymer Science, vol. 36, pp. 1697-1753, 2011.
  2. M. Kamkar, R. Salehiyan, T. Goudoulas, M. Abbasi, C. Saengow, E. Erfanian, S. Sadeghi, G. Natale, S. Rogers, A. Giacomin and U. Sundararaj, “Large amplitude oscillatory shear flow: Microstructural assessment of polymeric systems,” Progress in Polymer Science, vol. 132, p. 101580, 2022.
  3. S. Costanzo, D. Parisi, T. Schweizer and D. Vlassopoulos, “REVIEW: Nonlinear shear rheometry: Brief history, recent progress, and challenges,” Journal of Rheology, p. 1013–1036, 2024.
  4. A. Frank, “Evaluation of nonlinear LAOS experiments,” TA Instruments Applications Note, p. AAN031.
  5. T. Chen, “Using the Large Amplitude Oscillatory Shear (LAOS) Method to Characterize Polymer Long Chain Branching,” TA Instruments Application Note, p. RT006.
  6. A. Nakatani, S. Zhang, S. Ozair, A. Peera, W. Young, K. Kennedy, C. Peterson, C. Pearson and H. Ray, “Relationship between large amplitude oscillatory shear (LAOS) experiments and commercial pressure sensitive adhesives applications testing,” International Journal of Adhesion and Adhesives, vol. 108, p. 102869, 2021.
  7. M. Armstrong, A. Amaru, A. Zlotnik, A. Pincot, T. Brown and E. Milner, “Using rheological modeling and mechanical property analysis to interrogate, characterize, and develop metrics for human blood,” Results in Engineering, vol. 16, p. 100591, 2022.
  8. J. Sandoval, M. Fernández, O. Sanz, A. Santamaría, E. Penott-Chang and A. J. Müller, “Large amplitude oscillatory shear (LAOS) behavior of chocolates of different compositions,” Journal of Rheology, vol. 66, pp. 859-879, 2022.
  9. M. Anvari and H. Joyner, “Concentrated emulsions as novel fat replacers in reduced-fat and low-fat Cheddar cheeses. Part 2. Large amplitude oscillatory shear behavior,” International Dairy Journal, vol. 91, pp. 137-146, 2019.
  10. T. Ng, G. McKinley and R. Ewoldt, “Large amplitude oscillatory shear flow of gluten dough: A model power-law gel,” Journal of Rheology, vol. 55, pp. 627-654, 2011.
  11. K. Whitcomb, “Determining the Linear Viscoelastic Region in Oscillatory Measurements,” TA Instruments Applications Note, p. RH107.
  12. M. Wilhem, P. Reinheimer and M. Ortseifer, “High sensitivity Fourier-transform rheology,” Rheologica Acta, vol. 38, pp. 349-356, 1999.
  13. R. Ewoldt, A. Hosoi and G. McKinley, “New measures for characterizing nonlinear viscoelasticity in large amplitude oscillatory shear,” Journal of Rheology, vol. 52, p. 1427–1458, 2008.
  14. A. Le, M. Erturk, Y. Shim, S. Rogers and J. Kokini, “A critical study of the nonlinear rheological properties in major classes of foods using the Sequence of Physical Processes (SPP) method and the Fourier Transform Coupled with Chebyshev Decomposition (FTC) method,” Food Research International, vol. 174, p. 113587, 2023.
  15. R. Ewoldt and N. Bharadwaj, “Low-dimensional intrinsic material functions for nonlinear viscoelasticity,” Rheologica Acta, vol. 52, pp. 201-219, 2013.
  16. S. Chan, S. Varchanis, S. Haward and A. Shen, “Perspective on edge fracture,” Journal of Rheology, vol. 67, pp. 949-963, 2023.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This paper was written by Kimberly Dennis, PhD, Senior Applications Scientist.

TA Instruments, ARES-G3, and TRIOS are trademarks of Waters Corporation or its affiliates.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.