Keywords: thermal interface materials, phase change materials, TGA, DSC, TMA, dielectric, rheology, polyimide
TA502
Abstract
Isothermal crystallization kinetics was done on a commercially available machine screw made from polyether ether ketone (PEEK). The Avrami, Malkin, and Tobin macrokinetic models were utilized for crystallization from the melt and cold crystallization from the solid amorphous phase. Rate and geometric parameters were obtained, and the models fit the data well. The rate constants obtained from both the melt and solid amorphous were as expected. For crystallization from the melt, the geometric constants and Malkin C0 were consistent as a function of temperature. For cold crystallization of the solid amorphous phase, there was a temperature-dependent variation observed particularly in the Malkin C0 constant indicating a changing crystallization mechanism. Activation energies were obtained using the rate constants as well as an isoconversional method based on Friedman’s approach. For crystallization from the melt, activation energies were consistent showing good agreement with each of the models. Cold crystallization from the melt shows significant differences in activation energies obtained by the Avrami and Tobin models and the Malkin and isoconversional approach. Malkin and isoconversional show significantly lower activation energies of approximately 50 kJ/mol.
The equilibrium melting temperature was obtained from the crystallization data using the Hoffman-Weeks method. Lauritzen Hoffman parameters were obtained from the melt using the Malkin C1 rate constant as the growth parameter.
Isothermal crystallization kinetics is an important part of polymer characterization, yielding valuable information related to polymer processing. Isothermal crystallization kinetics correlates with material properties like modulus and optical clarity and can assess the effects of fillers and colorants, as well as the effect and optimization of chemical nucleators. Diagnostics of lot variations or competitive comparisons are also major uses of kinetic methodology in general and isothermal crystallization kinetics in particular.
Isothermal crystallization utilizing differential scanning calorimetry (DSC) is the most common approach for evaluating crystallization kinetics parameters. Crystallization can be evaluated from the melt amorphous phase or from the solid amorphous phase occurring during heating in the DSC experiment. Solid phase crystallization that occurs on heating is referred to as cold crystallization.
Crystallization of semi-crystalline polymers can be described as the sequence of two processes: primary and secondary crystallization. Primary crystallization relates to macroscopic development of crystallinity because of two consecutive microscopic mechanisms: primary and secondary nucleation (i.e. subsequent crystal growth).
Primary crystallization is assumed to cease when no additional molecular stems can transport onto a growth face and may be due to the impingement of crystalline aggregates onto one another. Secondary crystallization occurs after cessation of the primary process and may proceed in two ways: (1) crystal perfection of the primary lamellae and (2) crystallization of secondary lamellae from in the interstitial areas of the primary lamellae [1].
The fraction crystallized at time t is symbolized by X(t) and can be expressed as the fractional area under the exothermic curve in the DSC experiment and is described by Equation 1.

Where:
dHC/dt is the heat flow measured by the DSC
ΔHC is the total heat of crystallization.
Several macrokinetic models are used in isothermal crystallization kinetics. Some of the more common will be discussed here.
Avrami Model
The Avrami macrokinetic model (Equation 2) is most often used to describe isothermal crystallization kinetics of semi-crystalline polymers and is given by Equation 2.

Where:
X(t) = fraction crystallized as a function of time
ka = Avrami Rate Constant (function of nucleation and crystal growth rate)
na = Avrami Exponent (function of growth geometry)
t = time
Rearrangement yields the linear form of the Avrami equation:

A plot of the log (-ln(1-X(t)) versus log t is linear and yields the Avrami parameters ka and na and generally fits the data well between the limits of X(t) = 0.2 to X(t) = 0.8.
The crystallization half-time can be calculated from kA and nA using Equation 4.

Malkin Model
Malkin et. al. [2] proposed a different macrokinetic model based on the overall crystallization rate is dependent on the summation of the rate of primary nucleation and rate of crystal growth [3, 4]. The Malkin equation is shown in Equation 5.

Where:
X(t) fraction crystallized as a function of time
C0 is proportional to the ratio of secondary nucleation (linear growth) rate to the primary nucleation rate or specifically C0 ∝ G/I in Lauritzen and Hoffman terms
C1 is related to the overall crystallization rate or
C1 = aI + bG where a and b are constants.
The Avrami parameters n and k can be calculated from the Malkin constants.


Tobin Model
Tobin proposed an improvement to the Avrami model (which describes only the earliest stages of nucleation) [3] with a macrokinetic model that describes phase transformation kinetics with growth site impingement [5–7]. Tobin’s model is shown in Equation 8.

Where:
kT = Tobin rate constant
nT = Tobin exponent
The Tobin equation can be linearized and Tobin parameters nT and log of kT obtained as the slope and intercept of the line, respectively, using Equation 9 [4].

The crystallization activation energy can be calculated using the Arrhenius equation from the rate constants obtained from the models above as well as from the instantaneous crystallization rate as a function of conversion. The instantaneous crystallization rate was obtained using the protocols of ASTM E2070-3 [8].
According to Lauritzen and Hoffman theory, primary nucleation rate I and secondary nucleation or growth rate G are temperature dependent and can be described by Equations 10 and 11 [1].


Where I0 and G0 are pre-exponentials, U* is the activation energy for molecular transport across the melt/solid interfacial boundary given by the value of 6.276 kJ/mol, R is the universal gas constant, T∞ is the temperature where molecular motion ceases and for our purpose will be taken as thirty degrees below the glass transition temperature, ΔT = (TM0 − TC) where TM0 is the equilibrium melting temperature, f is a correction factor (given by Equation 12) KI and KG are combined factors related to primary nucleation and subsequent crystal growth, respectively, and given by Equation 12.

Where:
n = 4 for crystallization regimes I and III, and 2 for regime II
b = single layer thickness
σ = lateral surface free energy
σe = fold surface free energy
ΔHF = heat of fusion per unit volume
kB = the Boltzmann constant and f is a correction factor given as

where TM0 is the equilibrium melting temperature. For this work, the growth parameter G will be estimated using the Malkin rate constant C1.
The equilibrium melting temperature for the sample was determined using the Hoffman-Weeks method [9].
Sample
A commercially available machine screw made from PEEK was used for these experiments. A previous TGA investigation [10] determined that it contained 21.9% filler.
Instrument and Sample Preparation
The DSC experiment was performed using a TA Instruments™ Discovery™ DSC 2500 using nitrogen gas at a purge rate of 50 mL/min. Samples of 3 mg nominal mass were encapsulated using TZero™ Aluminum Pans. Each sample was used once to minimize any effects of thermal degradation.


Samples were heated to 400 °C and held isothermally to destroy process thermal history and any retained structural memory. Samples used in the cold crystallization experiment were quenched to induce as much solid amorphous phase as possible and heated and held at five different isothermal temperatures. The other samples were cooled from the melt to five different isothermal temperatures. Isothermal hold temperature information is summarized in Table 1.
Table 1. Isothermal hold temperatures for PEEK sample
| Run | Cold Crystallization Isothermal Temperature °C |
Cooling from melt Isothermal Temperature °C |
|---|---|---|
| 1 | 160 | 297 |
| 2 | 163 | 300 |
| 3 | 165 | 303 |
| 4 | 167 | 305 |
| 5 | 170 | 307 |
Data Reduction
Data sets were analyzed in the temperature ranges using the linearized form of the Avrami equation in the ranges of X(t) = 0.2 to 0.8. The entire data range was also analyzed using the Avrami, Malkin, and Tobin macrokinetic models. Activation energies were calculated from the rate constants obtained from the data fits. Activation energy as function of conversion was also calculated using an isoconversional approach similar to Friedman’s method from the raw DSC data. The Lauritzen and Hoffman parameters were calculated using the Malkin C1 rate constant for the growth rate parameter G.
Crystallization from the melt
Crystallization exotherms and integrations are shown in Figure 3 and Figure 4 respectively.


A comparison of the data obtained using the linear form of the Avrami equation is shown in Figure 5.
The rate constants calculated from the macrokinetic models are shown in Figure 6.


Table 2. Summary of kinetic parameters calculated from macrokinetic model fit of PEEK sample crystallized from the melt
| Temperature °C | Avrami Linear | Avrami | Malkin | Tobin | ||||
|---|---|---|---|---|---|---|---|---|
| nA | kA(min-n) | nA | kA(min-n) | C0 | C1(min-1) | nT | kT(min-n) | |
| 297 | 2.79 | 2.81 | 2.75 | 2.76 | 54.91 | 6.65 | 4.29 | 9.76 |
| 300 | 2.77 | 0.70 | 2.55 | 0.69 | 38.98 | 3.77 | 3.93 | 1.12 |
| 303 | 2.90 | 0.21 | 2.65 | 0.22 | 47.55 | 2.54 | 4.08 | 0.20 |
| 305 | 2.81 | 0.09 | 2.54 | 0.11 | 40.60 | 1.81 | 3.94 | 0.07 |
| 307 | 2.96 | 0.02 | 2.65 | 0.03 | 48.90 | 1.20 | 2.65 | 0.03 |
Geometric constants n and Malkin C0 calculated from the macrokinetic models are shown in Figure 7 stay constant throughout the experimental crystallization temperature range. The Avrami and Tobin n constant indicates a multi-dimensional growth geometry that remains consistent through the temperature range while the Malkin C0 parameter indicates consistent significant secondary crystal growth. The kinetic parameters for the cooling from the melt experiments are summarized in Table 2.
Activation energy using calculated rate constants
Crystallization activation energy was calculated using the rate constants calculated from the macrokinetic models and are summarized in Table 3.

Table 3. Summary of activation energies calculated from rate constants–crystallization from melt
| Rate constant (min-1) | Activation Energy (kJ/mol) | r2 |
|---|---|---|
| Avrami Linear (1/n) ln k | -442.3 | 0.996 |
| Avrami (1/n) ln k | -448.3 | 0.997 |
| Malkin C1 | -455.5 | 0.997 |
| Tobin (1/n) ln k | -480.1 | 0.987 |
Activation energy using an isoconversional method
The activation energy using the instantaneous crystallization rate from the DSC data at various levels of conversion is summarized in Table 4 and Figure 8. The activation energy calculated from the models yields a value of approximately -450 kJ / mol, the isoconversional method yields approximately -420 kJ on average. The drop in activation energy at X(t) = 0.7 (Figure 8) followed by the increase may indicate a regime change.
Table 4. Activation energy as function of conversion using isoconversional method – crystallization from melt
| X(t) | ΔE kJ mol-1 | R2 |
|---|---|---|
| 0.025 | -526.6 | 959 |
| 0.05 | -457.5 | 977 |
| 0.1 | -431.2 | 983 |
| 0.2 | -416.1 | 0.991 |
| 0.3 | -411.5 | 0.992 |
| 0.4 | -404.4 | 0.992 |
| 0.5 | -399.9 | 0.990 |
| 0.6 | -399.3 | 0.986 |
| 0.7 | -417.1 | 0.983 |
| 0.8 | -373.1 | 0.997 |
| 0.9 | -382.2 | 0.992 |

Determination of the equilibrium melting temperature (TM0)
TM0 was found to be 357.2 °C using the Hoffman-Weeks method and shown in Figure 9.
Lauritzen – Hoffman Analysis
Lauritzen – Hoffman analysis is plotted in Figure 10 and summarized in Table 5.
Table 5. Lauritzen Hoffman parameters for crystallization from melt
| U* (kJ/mol) | K(K2) | σσe(x104J/m4 | r2 |
|---|---|---|---|
| 6.276 | 365610 | 29.8 | 0.994 |
| 2.8 | 340958 | 27.8 | 0.994 |

Figure 9. Hoffman-Weeks determination of TM0

Crystallization from the Solid Amorphous Phase (Cold Crystallization)
Cold crystallization exotherms are shown in Figure 11. Fraction crystallized (X(t)) as a function of time is shown in Figure 12.
Avrami plots for the solid amorphous cold crystallization are shown in Figure 13. The sample held at 167 °C shows more deviation from linearity than the other samples, including the higher temperature 170 °C, which may indicate a narrow range temperature dependent regime change.
The rate constants, geometric constants, and Malkin C0 are summarized in Table 6, the rate constants are shown in Figure 14, and the geometric constants n and Malkin C0 are shown in Figure 15. As observed in the linear Avrami plot shown in Figure 13, there is a temperature dependent regime change most evident at 167 °C. The Malkin constant C0, which is proportional to the ratio of secondary to primary crystallization, drops as the crystallization temperature increases, reaching an apparent minimum of 11.6 at 167 °C, followed by an upward trend at 170 °C.




Table 6. Summary of kinetic parameters calculated from macrokinetic model fit of PEEK sample cold crystallized from solid amorphous
| Temperature °C | Avrami Linear | Avrami | Malkin | Tobin | ||||
|---|---|---|---|---|---|---|---|---|
| nA | kA(min-n) | nA | kA(min-n) | C0 | C1(min-1) | nT | kT(min-n) | |
| 160 | 2.94 | 0.004 | 2.81 | 0.005 | 59.88 | 0.730 | 4.35 | 0.001 |
| 163 | 2.57 | 0.065 | 2.35 | 0.079 | 27.52 | 1.333 | 3.68 | 0.037 |
| 165 | 2.52 | 0.302 | 2.32 | 0.320 | 26.20 | 2.377 | 3.66 | 0.332 |
| 167 | 2.27 | 1.368 | 1.90 | 1.202 | 11.61 | 3.446 | 3.03 | 2.675 |
| 170 | 2.47 | 4.479 | 2.16 | 3.502 | 19.56 | 6.447 | 3.37 | 14.017 |
Activation energies calculated from the obtained rate constants are shown in Table 7. The activation energies obtained using the Avrami and Tobin models yield a value of approximately 400 kJ/mol, contrasted with the Malkin C1 rate constant and most of the range of the isoconversional method, which yield a value of approximately 350 kJ/mol.

Figure 15. Geometric constants n and Malkin C0 from macrokinetic models – cold crystallization from solid amorphous, (Malkin C0 plotted on secondary y-axis)
Table 7. Activation energies calculate from rate constants
| Rate constant (min-1) | Activation Energy (kJ/mol) | r2 |
|---|---|---|
| Avrami Linear (1/n) ln k | 405.0 | 0.994 |
| Avrami (1/n) ln k | 400.8 | 0.995 |
| Malkin C1 | 351.9 | 0.998 |
| Tobin (1/n) ln k | 409.1 | 0.993 |
Activation energies calculated using the isoconversional method are summarized in Table 8 and shown in Figure 16. The onset of crystallization shows an activation energy of approximately 300 kJ/mol, converging to an average value of 365 kJ/mol from X(t) 0.1 to 0.7 with a significant reduction to 313 and 226 kJ/mol at X(t) 0.8 and 0.9, respectively. The late-stage reduction in activation energy is due to a changing crystallization mechanism (interstitial nucleation) caused by heat flow impingement of the developing nuclei.
Cold crystallization kinetics of the solid amorphous phase show different results than crystallization from the melt. The Avrami and Tobin geometric constants (n) decrease slightly with temperature indicating a temperature dependent change in nucleation geometry from spherical to more planar. The Malkin C0 constant also decreases and minimizes at 167 °C at a value of 11.6, indicative of more primary crystallization occurring. As expected, the rate constants show normal Arrhenius behavior. Data fits of the models are good.
Because of the elevated temperature uses of PEEK, it is important to evaluate the kinetics of cold crystallization and potential effects on material properties as amorphous phase induced during processing crystallizes on heating during service. Even at modest service temperatures, enthalpic relaxation of the amorphous phase may also affect properties and can also be evaluated using DSC in another experimental design. The sample screw used in this analysis does show cold crystallization and some enthalpic recovery [10].
Table 8. Activation energy of cold crystallization using iso conversional method cold crystallized from solid amorphous
| X(t) | ΔE kJ mol-1 | R2 |
|---|---|---|
| 0.025 | 298.7 | 0.884 |
| 0.05 | 329.2 | 0.960 |
| 0.1 | 349.1 | 0.986 |
| 0.2 | 366.5 | 0.992 |
| 0.3 | 372.5 | 0.993 |
| 0.4 | 375.9 | 0.995 |
| 0.5 | 375.3 | 0.995 |
| 0.6 | 365.0 | 0.994 |
| 0.7 | 347.8 | 0.994 |
| 0.8 | 312.9 | 0.978 |
| 0.9 | 226.1 | 0.919 |

The purpose of this work is to demonstrate the workflow in obtaining isothermal crystallization kinetics of a polymer sample that might be submitted to an analytical laboratory for characterization. Isothermal crystallization kinetics is an important part of polymer characterization that yields information related to prediction and optimization of polymer processing, correlating with material properties like modulus and optical clarity, assessing effects of fillers and colorants, and effect and optimization of chemical nucleators. Diagnostics of lot variations or competitive comparisons are also uses of kinetic methodology in general and isothermal crystallization kinetics in particular. The results of this work demonstrate that the Discovery 2500 DSC with TZero Technology is a useful and valuable tool for obtaining high quality data to perform sophisticated kinetics measurements.
Isothermal kinetics of a machine screw made from reinforced PEEK of the melt phase and solid amorphous phase were determined using common macrokinetic models. Kinetic information from crystallization from the melt shows consistent results from the three models used with the Avrami and Tobin nucleation constants n consistent as a function of temperature and indicating a spherulitic growth geometry. The Malkin C0 constant shows consistently high secondary growth as a function of temperature. The activation energies calculated from the rate constants show good agreement and the expected anti-Arrhenius behavior, but the isoconversional method shows a significant drop between X(t) = 0.7 and 0.8 followed by a sharp increase, which is likely due to a regime change. The Malkin C1 rate constant was used to calculate the Lauritzen-Hoffman parameters and shows good linearity with the model.
This DSC experiment shows that this PEEK sample crystallizes from the melt in a consistent, predictable way. Cold crystallization from the solid amorphous phase shows temperature-dependent nucleation mechanisms evident in the Avrami and Tobin geometric constants (n) and the Malkin C0 parameter. It is likely that metastable amorphous phase will be introduced into the structure during processing and with potential high service temperatures in PEEK, crystallization may occur which may affect end-use properties like modulus and impact resistance. Enthalpic relaxation of the amorphous phase is also a possibility and can be assessed with other types of DSC experiments. Evaluation of modulus and impact resistance can be evaluated by dynamic mechanical analysis (DMA) and established physical testing methods.
The TA Instruments Discovery 2500 DSC with TZero Technology is useful and valuable tool for obtaining high quality data to perform sophisticated kinetics measurements.
Sections
Common Macrokinetic Models Used in Isothermal Crystallization Kinetics
Equilibrium Melting Temperature
Related Resources
References
- P. Supaphol and J. Spruiell, “Isothermal melt- and coldcrystallization kinetics and subsequent melting behavior in syndiotactic polypropylene: a differential scanning calorimetry study,” Polymer, vol. 42, pp. 699-712, 2001.
- Y. Malkin and V. Beghishev, “General Treatment of Polymer Crystallization Kinetics – Part 1. A New Macrokinetic Equation and its Experimental Validation,” Polymer Engineering and Science, vol. 24, no. 18, pp. 1396-1401, 1984.
- P. Supaphol and J. Spruiell, “Application of the Avrami, Tobin, Malkin, and Simultaneous Avrami Macrokinetic Models to Isothermal Crystallization of Syndiotactic Polpropylenes,” Journal of Macromolecular Science and Physics, vol. B(39)2, pp. 257-277, 2000.
- C. Kelly and M. Jenkins, “Modeling the Crystallization Kinetics of Polymers Displaying High Levels of Secondary Crystallization,” Polymer Journal, vol. 54, pp. 249-257, 2022.
- M. Tobin, “Theory of Phase Transition Kinetics with Growth Site Impingement. I. Homogeneous Nucleation,” Journal of Polymer Science – Polymer Physics, vol. 12, no. 2, pp. 399-406, 1974.
- M. Tobin, “The Theory of Phase Change Kinetics with Growth Site Impingement. II. Hetergeneous Nucleation,” Journal of Polymer Science – Polymer Physics , vol. 14, no. 12, pp. 2253-2257, 1976.
- M. Tobin, “Theory of Phase Transition Kinetics with Growth Site Impingement. III. Mixed Hetergeneous-Homogeneous Nucleation and Nonintegtral Expnents of Time,” Journal of Polymer Science – Polymer Physics , vol. 15, no. 12, pp. 2269-2270, 1977.
- ASTM, E 2070-03: Standard Test Method for Kinetic Paramters by Differential Scanning Calorimetry Using Isothermal Methods, Conshohocken, PA: ASTM, 2003.
- J. Hoffman and J. Weeks, “Melting Process and the Equilibrium Melting Temperature of Polychlorotrifluroethylene,” Journal of Research of the National Bureau of Standards, vol. 66A, no. No. 1, pp. 13-28, January – February 1962.
- Browne, J.A., Thermal Analysis of Polyether ether ketone – Application Note: TA496, 2025.
Acknowledgement
For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.
Thank you to Radek Osborn for preparing the samples used in this investigation.
This paper was written by James Browne, applications scientist at Waters Corporation.
TA Instruments, Discovery, and TZero are trademarks of Waters Corporation or its affiliates.
Click here to download the printable version of this application note.