Determination of the Linear Viscoelastic Region for Solid Bar Samples

Keywords: dynamic mechanical analysis (DMA); linear viscoelastic region; 3-point bending; cantilever clamp

TB119

Abstract

Determination of the linear viscoelastic region (LVR) is a fundamental prerequisite for dynamic mechanical measurements. Within the LVR, the material response is linear, meaning that stress is proportional to strain and the measured viscoelastic properties depend only on temperature and time (or frequency), not on the magnitude of deformation. Dynamic mechanical analysis techniques such as frequency sweeps, temperature ramps, and certain static tests, including stress relaxation, rely on this assumption of linearity to ensure that the measured moduli reflect intrinsic material behavior rather than traits arising from non‑linear deformation. This technical brief describes a methodology for determining the LVR of solid bar specimens using a TA Instruments™ Discovery™ DMA 850.

Introduction

The linear viscoelastic region (LVR) [1, 2] is defined as the range of strain or stress amplitudes over which the measured viscoelastic properties, particularly the storage modulus (E′), are independent of deformation amplitude. Three-point bending and single or dual cantilever clamps are well suited for determining the LVR of solid bar samples. Three-point bending is preferred when high sensitivity to small deformations is required. With this clamp, the maximum strain is localized at the sample midpoint, thus making it especially suitable for stiff materials. Single and dual cantilever clamps apply a more distributed bending moment along the sample and, due to rigid clamping, provide greater mechanical stability at larger deformation amplitudes. This makes these cantilevers particularly suitable for softer solids, viscoelastic polymers, or materials prone to cracking under point loading. These clamps, along with the DMA 850, are shown in Figure 1. Together, they enable robust determination of the LVR across a wide range of material stiffnesses.

Figure 1. a) DMA 850 b) 3-point bending c) Dual cantilever
Figure 1. a) DMA 850 b) 3-point bending c) Dual cantilever

This Technical Brief describes best practices for obtaining reproducible modulus measurements and for determining the linear viscoelastic region (LVR) as the basis for reliable dynamic testing of solid bar samples using three-point bending and cantilever clamps on the DMA 850.

Experimental, Results, and Discussion

Three-Point Bending

To perform strain amplitude sweeps for LVR determination in 3-point bending, an appropriate preload (static force) is required to maintain continuous mechanical contact between the sample and the clamp throughout oscillatory deformation. Because the sample is not rigidly clamped, insufficient preload can result in intermittent loss of contact during parts of the oscillation cycle, leading to underestimation of the storage modulus (E′) or premature termination of the test. In contrast, excessive preload induces static bending strain that can artificially inflate the measured modulus, especially at lower strain levels. Therefore, preload must be carefully optimized and set to the lowest value that ensures stable, repeatable modulus measurements without inducing nonlinear deformation.

Force Tracking

Force tracking is an essential feature of the DMA 850 that, when used in addition to preload, helps ensure reliable and reproducible measurements of viscoelastic properties. It is defined as the ratio of the static (axial) force to the dynamic (oscillatory) force applied during a test and is always greater than unity (greater than 100%). When force tracking is enabled, the instrument automatically adjusts the static force to maintain a user-defined percentage above the oscillation force required to drive the sample at the programmed amplitude of strain or stress. This ensures continuous contact between the sample and the movable clamp during oscillatory testing, even as material stiffness changes with temperature or frequency, such as:

  • Temperature ramps: Force tracking is recommended because material stiffness changes significantly during heating or cooling. As a material softens during heating, the oscillation force decreases; force tracking automatically reduces the axial force proportionally while keeping it above the oscillation force by the programmed percentage. For example, with force tracking set to 125%, the DMA 850 maintains the axial force at 125% of the oscillation force. As stiffness decreases, both forces decrease together, ensuring continuous contact without applying unnecessary strain.
  • Frequency sweeps: Force tracking can serve as a safety measure, particularly when targeting very high frequencies (e.g., 100 Hz), where dynamic forces may fluctuate more strongly.
  • When force tracking is not recommended: Many researchers prefer to keep the axial force constant to minimize the number of varying parameters in their study. When comparing modulus values, it is generally preferable to maintain consistent frequency, temperature, and axial force across all measurements. In such cases, force tracking should be disabled.

Preload / Force Tracking Determination Procedure

To begin testing an unknown sample and to determine its modulus and linear viscoelastic region (LVR), a systematic approach is required because the material stiffness and contact behavior are not known a priori. The following procedure is recommended:

  1. Begin with a moderate initial preload (e.g., 1 N).
  2. Enable force tracking to maintain continuous contact between the sample and the clamp during oscillatory deformation. Start with a moderate force tracking ratio, such as 125%.
  3. With preload and force tracking engaged, perform a strain amplitude sweep.
  4. Monitor the storage modulus (E′), oscillation force, and axial force throughout the test.

Because solid bar samples typically do not have perfectly flat or parallel surfaces, increasing the axial force often results in an increase in the measured storage modulus (E′) due to improved contact between the sample and the clamp (Figure 2). The minimum required preload is identified as the lowest axial force at which E′ becomes nearly independent of axial force, indicating stable and continuous contact throughout the oscillation cycle. Applying a preload beyond this value provides no additional benefit and should be avoided. Once the appropriate preload is identified for a specific sample, it is fixed and used for all subsequent DMA measurements.

When a strain amplitude sweep at 1 Hz was performed on Bar #1, the storage modulus (E′) became effectively independent of axial force at approximately 6 N, as shown in Figure 2. This behavior indicates that stable and sufficient contact had been achieved between the sample and the clamp.

To further validate this behavior, force tracking was disabled and the same amplitude sweep test was conducted at lower axial forces. Under these conditions, loss of contact was observed as the strain amplitude increased, resulting in premature termination of the amplitude sweep (Figure 3).

Figure 2. LVR of Bar #1– 1 N pre-load and 125% force tracking
Figure 2. LVR of Bar #1– 1 N pre-load and 125% force tracking
Figure 3. LVR at different pre-load values – no force tracking - Bar #1
Figure 3. LVR at different pre-load values – no force tracking - Bar #1

Based on the storage modulus plateau observed at a preload of 6 N in Figures 2 and 3, a strain amplitude of 0.006% can be selected as being well within the linear viscoelastic region (LVR) for subsequent tests. At this condition, we maintain almost stable contact between the clamp and the sample, and the modulus remains quite steady. In addition, the pre‑load was minimized to the lowest appropriate axial force, out of the instrument’s maximum force limit of 18 N, which leaves more room for further dynamic tests, especially for such a stiff material.

It is also observed that if lower pre-loads are preferred, the strain amplitude must be reduced accordingly. However, at extremely low strain levels, the signal-to-noise ratio becomes poor, making it difficult to obtain reliable data in subsequent dynamic tests.

The same preload determination and amplitude sweep procedure was applied to Bar #2, a less stiff material. For this material, a preload of 4 N was identified as the lowest axial force that provided a stable storage modulus (E′), indicating continuous and reliable contact throughout oscillation (Figure 4).

Based on the amplitude sweep results, a strain amplitude of 0.06% was identified to lie within the linear viscoelastic region (LVR) for Bar #2 and could be selected for subsequent dynamic measurements (Figure 5).

Figure 4. LVR determination for Bar #2– axial force
Figure 4. LVR determination for Bar #2– axial force
Figure 5. Strain from LVR for Bar #2 - pre-loads with and without force tracking
Figure 5. Strain from LVR for Bar #2 - pre-loads with and without force tracking

In both cases, the modulus measured within the strain amplitude range where it is independent of strain, is found to be reproducible and suitable for reporting in datasheets or similar technical documents.

Elevated Temperature Effects on LVR Determination

When DMA measurements are performed at elevated temperatures, two competing effects must be considered during LVR determination. As temperature increases, the material typically becomes softer and more compliant, which extends the linear viscoelastic region (LVR) to higher strain amplitudes. This expansion of the LVR is advantageous, as it allows larger deformation amplitudes to be applied while maintaining linear response. However, this same softening also reduces the measured force response at low strain amplitudes, which can result in weaker signals and increased noise, particularly near the lower end of the LVR.

Additionally, as the material softens at higher temperatures, sagging becomes increasingly significant in 3-point bending geometry. Excessive sag can compromise contact, reduce measurement stability, or make it impractical to maintain the required preload or required applied strain. For this reason, 3-point bending may no longer be suitable for low-stiffness materials at elevated temperatures. Accordingly, for Bar #2, which exhibits lower stiffness, the dual cantilever clamp was also employed to determine the LVR, as clamped geometries are less sensitive to sagging and provide more stable contact under softened conditions.

Dual/Single Cantilever Bending

In contrast to 3-point bending, cantilever clamps do not rely on contact preload for force transmission, as the sample is rigidly clamped. Consequently, the preload-related increase in storage modulus associated with improved contact is generally absent. As shown in Figure 6, the modulus in cantilever remains stable at low strain amplitudes and deviates only upon departure from the linear viscoelastic region.

In this work, the LVR is defined as the strain range over which the storage modulus (E’) changes by no more than 5% relative to its low-strain plateau value, a commonly used and practical criterion for identifying the onset of nonlinearity.

As shown in Figure 7, the linear viscoelastic region (LVR) can be readily identified using dual cantilever clamp at 100 °C. A wide LVR is observed, providing flexibility in strain selection. The strain value of 0.06 % could be subsequently used for further dynamic measurements to ensure linear viscoelastic response.

Figure 6. LVR determination for Bar #2 using dual cantilever clamp – Room temperature
Figure 6. LVR determination for Bar #2 using dual cantilever clamp – Room temperature
Figure 7. LVR determination for Bar #2 using dual cantilever clamp – 100 °C
Figure 7. LVR determination for Bar #2 using dual cantilever clamp – 100 °C

Bar #2 cannot be reliably tested in 3-point bending because the material softens at elevated temperatures and undergoes sagging when the movable clamp contacts the already softened sample and attempts to apply the commanded strain, leading to loss of contact between the sample and the clamp, resulting in unstable measurements and test failure (Figure 8).

Figure 8. The bar #2 at 100 °C was tested using 3-point bending - the amplitude sweep.
Figure 8. The bar #2 at 100 °C was tested using 3-point bending - the amplitude sweep.

Conclusions

This technical brief demonstrates a systematic methodology for determining the linear viscoelastic region (LVR) and obtaining reproducible modulus measurements for solid bar samples using the Discovery DMA 850. By carefully optimizing preload and judiciously applying force tracking in 3-point bending, stable sample–clamp contact can be ensured without inducing nonlinear deformation.

The choice of test clamp is shown to be critical, particularly at elevated temperatures where material softening and sagging may compromise 3-point bending measurements. In such cases, rigidly clamped cantilever geometries offer superior stability and reliability. Overall, the practices outlined here enable robust selection of test conditions and improve the accuracy and confidence of dynamic mechanical measurements across a wide range of material stiffnesses.

References

  1. TA Instruments, “RH107: Determining the Linear Viscoelastic Region in Oscillatory Measurements,” [Online]. Available: https://www.tainstruments.com/applications-notes/determining-thelinear-viscoelastic-region-in-oscillatory-measurements/.
  2. TA Instruments, “Basics of Rheology Episode 3,” [Online]. Available: https://www.youtube.com/watch?v=hgUDHyA4sP8&t=344s.

Acknowledgement

For more information or to request a product quote, please visit www.tainstruments.com to locate your local sales office information.

This Technical Brief was written by Behbood Abedi, PhD., application scientist at Waters Corporation.

TA Instruments and Discovery are trademarks of Waters Corporation or its affiliates.

Click here to download the printable version of this application note.

Contact us to learn more about our instrumentation and how it can benefit your research.